===[[Process Group - Process Control Data#Deposition .28Process Control Data.29|<u>Process Control Data</u>]]===
{{Recipe Table Explanation}}
<small>''See [[Process Group - Process Control Data#Deposition .28Process Control Data.29|linked page]] for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.''</small>
{| border="1" class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;"

|- bgcolor="#D0E7FF"
===Deposition Tools/Materials Table===
! width="1675" height="45" colspan="18" | <div style="font-size: 150%;">Vacuum Deposition Recipes</div>

|- bgcolor="#D0E7FF"
==== Process Maturity Ranking ====
| <!-- INTENTIONALLY LEFT BLANK --> <br>

! bgcolor="#D0E7FF" align="center" colspan="4" | '''[[E-Beam Evaporation Recipes|E-Beam Evaporation]]'''
* <code>'''R6'''</code> - most mature process with regular calibrations recorded on SPC charts.
! bgcolor="#D0E7FF" align="center" colspan="6" | '''[[Sputtering Recipes|Sputtering]]'''
* …
! bgcolor="#D0E7FF" align="center" colspan="2" | '''[[Thermal Evaporation Recipes|Thermal Evaporation]]'''
* <code>'''R1'''</code> - least mature - "possible" but you'll have to figure it out.
! bgcolor="#D0E7FF" align="center" colspan="3" | '''[[PECVD Recipes|Plasma Enhanced Chemical<br>Vapor Deposition (PECVD)]]'''

! width="90" bgcolor="#D0E7FF" align="center" | '''[[Atomic Layer Deposition Recipes|Atomic Layer Deposition]]'''
''The Key/Legend for this table's <code>R1...R6</code> values is at the [[Vacuum Deposition Recipes#Process Ranking Table|<u>bottom of the page</u>]].''
! width="80" bgcolor="#D0E7FF" align="center" | '''[[Molecular Vapor Deposition Recipes|Molecular Vapor Deposition]]'''
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1"
|- bgcolor="#d0e7ff"
! colspan="16" width="1675" height="45" |<div style="font-size: 150%;">Vacuum Deposition Recipes</div>
|- bgcolor="#d0e7ff"
|<!-- INTENTIONALLY LEFT BLANK --><br>
! colspan="4" bgcolor="#d0e7ff" align="center" |'''[[E-Beam Evaporation Recipes|E-Beam Evaporation]]'''
! colspan="4" |'''[[Sputtering Recipes|Sputtering]]'''
! colspan="2" bgcolor="#d0e7ff" align="center" |'''[[Thermal Evaporation Recipes|Thermal Evaporation]]'''
! colspan="3" bgcolor="#d0e7ff" align="center" |'''[[PECVD Recipes|Plasma Enhanced Chemical<br>Vapor Deposition (PECVD)]]'''
! width="90" bgcolor="#d0e7ff" align="center" |'''[[Atomic Layer Deposition Recipes|Atomic Layer Deposition]]'''
! width="80" bgcolor="#d0e7ff" align="center" |'''[[Molecular Vapor Deposition Recipes|Molecular Vapor Deposition]]'''
|-
|-
! width="20" bgcolor="#D0E7FF" align="center" | '''Material'''
! width="20" bgcolor="#d0e7ff" align="center" |'''Material'''
| width="65" bgcolor="#DAF1FF" | [[E-Beam Evaporation Recipes#E-Beam_1_.28Sharon.29|E-Beam 1 (Sharon)]]
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_1_.28Sharon.29|E-Beam 1 (Sharon)]]
| width="65" bgcolor="#DAF1FF" | [[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]]
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]]
| width="65" bgcolor="#DAF1FF" | [[E-Beam Evaporation Recipes#E-Beam_3_.28Temescal.29|E-Beam 3 (Temescal)]]
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_3_.28Temescal.29|E-Beam 3 (Temescal)]]
| width="65" bgcolor="#DAF1FF" | [[E-Beam Evaporation Recipes#E-Beam_4_.28CHA.29|E-Beam 4 (CHA)]]
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_4_.28CHA.29|E-Beam 4 (CHA)]]
| width="65" bgcolor="#DAF1FF" | [[Sputtering Recipes#Sputter_1_.28Custom.29|Sputter 1 (Custom)]]
| width="65" bgcolor="#daf1ff" |[[Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29|Sputter 3<br>(AJA ATC 2000-F)]]
| width="65" bgcolor="#DAF1FF" | [[Sputtering Recipes#Sputter_2_.28SFI_Endeavor.29|Sputter 2<br>(SFI Endeavor)]]
| width="65" bgcolor="#daf1ff" |[[Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29|Sputter 4<br>(AJA ATC 2200-V)]]
| width="65" bgcolor="#DAF1FF" | [[Sputtering Recipes#Sputter_3_.28ATC_2000-F.29|Sputter 3<br>(ATC 2000-F)]]
| width="65" bgcolor="#daf1ff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_5_.28AJA_ATC_2200-V.29 Sputter 5 (AJA ATC 2200-V)]
| width="65" bgcolor="#DAF1FF" | [[Sputtering Recipes#Sputter_4_.28ATC_2200-V.29|Sputter 4<br>(ATC 2200-V)]]
| width="55" bgcolor="#daf1ff" |[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|Ion Beam<br>Deposition (Veeco Nexus)]]
| width="65" bgcolor="#DAF1FF" | [[Sputtering Recipes#Sputter_5_.28Lesker_AXXIS.29|Sputter 5 (Lesker AXXIS)]]
| width="45" bgcolor="#daf1ff" |[[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]]
| width="55" bgcolor="#DAF1FF" | [[Ion Beam Deposition (Veeco NEXUS)|Ion Beam<br>Deposition (Tool)]]
| width="65" bgcolor="#daf1ff" |[[Thermal Evaporation Recipes#Thermal_Evap_2_.28Solder.29|Thermal Evap 2 (Solder)]]
| width="45" bgcolor="#DAF1FF" | [[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]]
| width="65" bgcolor="#daf1ff" |[[PECVD Recipes#PECVD_1_.28PlasmaTherm_790.29|PECVD 1<br>(PlasmaTherm 790)]]
| width="65" bgcolor="#DAF1FF" | [[Thermal Evaporation Recipes#Thermal_Evap_2_.28Solder.29|Thermal Evap 2 (Solder)]]
| width="65" bgcolor="#daf1ff" |[[PECVD Recipes#PECVD_2_.28Advanced_Vacuum.29|PECVD 2<br>(Advanced Vacuum)]]
| width="65" bgcolor="#DAF1FF" | [[PECVD Recipes#PECVD_1_.28PlasmaTherm_790.29|PECVD 1<br>(PlasmaTherm 790)]]
| width="65" bgcolor="#daf1ff" |[[PECVD_Recipes#ICP-PECVD_.28Unaxis_VLR.29|Unaxis VLR ICP-PECVD]]
| width="65" bgcolor="#DAF1FF" | [[PECVD Recipes#PECVD_2_.28Advanced_Vacuum.29|PECVD 2<br>(Advanced Vacuum)]]
| width="65" bgcolor="#daf1ff" |[[Atomic_Layer_Deposition_Recipes|Atomic Layer Deposition (Oxford FlexAL)]]
| width="65" bgcolor="#DAF1FF" | [[PECVD Recipes#Unaxis_VLR_ICP-PECVD|Unaxis VLR ICP-PECVD]]
| width="65" bgcolor="#daf1ff" |[[Molecular Vapor Deposition|Molecular Vapor Deposition (Tool)]]
| width="65" bgcolor="#DAF1FF" | [[Atomic Layer Deposition (Oxford FlexAL)|Atomic Layer Deposition (Tool)]]
| width="65" bgcolor="#DAF1FF" | [[Molecular Vapor Deposition|Molecular Vapor Deposition (Tool)]]
|-
|-
! bgcolor="#D0E7FF" align="center" | Ag
! bgcolor="#d0e7ff" align="center" |Ag
| bgcolor="EEFFFF" | {{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{Al/E3}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="EEFFFF" | {{Al/E4}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | [[Sputtering Recipes|A]]
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | [[Sputtering Recipes|A]]
| bgcolor="#eeffff" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
!AgBr
! bgcolor="#D0E7FF" align="center" | Al
|
| {{Al/E1}}
|
| <br>
|
| {{Al/E3}}
|
| {{Al/E4}}
|
| <br>
|
| {{rl|Sputtering Recipes|Al deposition (Sputter 2)}}
|
| [[Sputtering Recipes|A]]
|
| [[Sputtering Recipes|R]]
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
| <br>
| <br>
|-
|-
!AgCl
! bgcolor="#D0E7FF" align="center" | Al<sub>2</sub>O<sub>3</sub>
|
| bgcolor="EEFFFF" | {{Al/E1}}
|
| bgcolor="EEFFFF" | {{Al/E2}}
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | [[Ion_Beam_Deposition_(Veeco_NEXUS)|A]]
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | {{rl|Atomic Layer Deposition Recipes|Al2O3 deposition (ALD)}}
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | AlN
! bgcolor="#d0e7ff" align="center" |Al
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| <br>
| <br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| <br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| <br>
|[[Sputtering Recipes|R1]]
| <br>
| {{rl|Sputtering Recipes|AlN deposition (Sputter 2)}}
|[[Sputtering Recipes|R3]]
|[[Sputtering Recipes|R6]]
| <br>
|R1
| <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
| <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
| [[Ion_Beam_Deposition_(Veeco_NEXUS)|A]]
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| {{rl|Atomic Layer Deposition Recipes|AlN deposition (ALD)}}
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Au
! bgcolor="#d0e7ff" align="center" |Al<sub>2</sub>O<sub>3</sub>
| bgcolor="EEFFFF" | {{Al/E1}}
| bgcolor="#eeffff" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
| bgcolor="EEFFFF" | {{Al/E3}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{Al/E4}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="EEFFFF" | {{rl|Sputtering Recipes|Au deposition (Sputter 2)}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="EEFFFF" | [[Sputtering Recipes|A]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | {{rl|Sputtering Recipes|Ti-Au Deposition (Sputter 4)}}
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R3]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Al2O3 deposition .28ALD CHAMBER 3.29|R3]]
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
!AuPd
! bgcolor="#D0E7FF" align="center" | B
|R1
| <br>
|
| <br>
|
| <br>
|R1
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
| <br>
| <br>
|-
|-
!AuZn
! bgcolor="#D0E7FF" align="center" | Co
|
| bgcolor="EEFFFF" | {{Al/E1}}
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | {{Al/E4}}
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | [[Sputtering Recipes|A]]
|
| bgcolor="EEFFFF" | <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
!AuSn
! bgcolor="#D0E7FF" align="center" | Cr
|
| <br>
|
| <br>
|
| <br>
|
| {{Al/E4}}
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
| <br>
| <br>
|-
|-
!AuGe
! bgcolor="#D0E7FF" align="center" | Cu
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|R1
| bgcolor="EEFFFF" | <br>
|R2
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Fe
! bgcolor="#d0e7ff" align="center" |AlN
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
|<br>
| {{Al/E4}}
|[[Sputtering Recipes|R1]]
| <br>
|[[Sputtering Recipes|R1]]
| <br>
|<br>
| [[Sputtering Recipes|A]]
|R1
| <br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29|R3]]
| <br>
| <br>
|<br>
| <br>
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Ge
! bgcolor="#d0e7ff" align="center" |Au
| bgcolor="EEFFFF" | {{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R6]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{Al/E3}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Au|R6]]
| bgcolor="EEFFFF" | {{Al/E4}}
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |R2
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |R3
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | GeO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |B
|<br>
|
|<br>
| {{Al/E2}}
|<br>
|
|<br>
|
|<br>
|
|<br>
|
|<br>
|
|<br>
|
|<br>
|
|
|
|<br>
|
|<br>
|
|<br>
|
|<br>
|
|<br>
|
|
|
|-
|-
! bgcolor="#D0E7FF" align="center" | Gd
! bgcolor="#d0e7ff" align="center" |C
| bgcolor="#eeffff" align="center" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R3]]
| bgcolor="EEFFFF" | {{Al/E1}}
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | {{Al/E4}}
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" align="center" |
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
!CaF2
! bgcolor="#D0E7FF" align="center" | Hf
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | {{Al/E4}}
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | HfO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |CeO<sub>2</sub>
| <br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R3]]
| <br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| {{rl|Atomic Layer Deposition Recipes|HfO2 deposition (ALD)}}
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | In
! bgcolor="#d0e7ff" align="center" |Co
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Ir
! bgcolor="#d0e7ff" align="center" |Cr
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R6]]
| <br>
| <br>
|<br>
| <br>
|R2<br>
|[[Process Group - Process Control Data#E-Beam 4: Cr|R6]]
| {{Al/E4}}
|[https://wiki.nanotech.ucsb.edu/w/index.php?title=Sputtering_Recipes#Sputter_3_.28AJA_ATC_2000-F.29 R3]
| <br>
| <br>
|<br>
|{{Rl|Sputtering_Recipes|Sputter_5_.28AJA_ATC_2200-V.29|R6}}
| <br>
| <br>
|<br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
| <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
| <br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | ITO
! bgcolor="#d0e7ff" align="center" |Cu
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
| bgcolor="EEFFFF" | {{Al/E2}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R2]]
| bgcolor="EEFFFF" | [[Ion_Beam_Deposition_(Veeco_NEXUS)|A]]
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | MgO
! bgcolor="#d0e7ff" align="center" |Fe
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
|
|<br>
| {{Al/E2}}
|<br>
|
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
|
|[[Sputtering Recipes|R3]]
|
|<br>
|
|<br>
|
|<br>
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
|
|<br>
|
|<br>
|
|<br>
|
|<br>
|
|<br>
|
|
|
|-
|-
! bgcolor="#D0E7FF" align="center" | Mo
! bgcolor="#d0e7ff" align="center" |Ge
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>R2
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Nb
! bgcolor="#d0e7ff" align="center" |GeO<sub>2</sub>
|
| <br>
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]]
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| [[Sputtering Recipes|R]]
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
| <br>
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Ni
! bgcolor="#d0e7ff" align="center" |Gd
| bgcolor="EEFFFF" | {{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{Al/E3}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{Al/E4}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{rl|Sputtering Recipes|Ni deposition (Sputter 3)}}
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | NiCr
! bgcolor="#d0e7ff" align="center" |Hf
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]]
| {{Al/E4}}
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
| bgcolor="#eeffff" |<br>
|
|
|
|-
|-
! bgcolor="#D0E7FF" align="center" | NiFe
! bgcolor="#d0e7ff" align="center" |HfO<sub>2</sub>
|<br>
| bgcolor="EEFFFF" |
|<br>
| bgcolor="EEFFFF" |
|<br>
| bgcolor="EEFFFF" |
|<br>
| bgcolor="EEFFFF" | {{Al/E4}}
|
| bgcolor="EEFFFF" |
|
| bgcolor="EEFFFF" |
|R1
| bgcolor="EEFFFF" | [[Sputtering Recipes|A]]
|<br>
| bgcolor="EEFFFF" |
|<br>
| bgcolor="EEFFFF" |
|<br>
| bgcolor="EEFFFF" |
|<br>
| bgcolor="EEFFFF" |
|<br>
| bgcolor="EEFFFF" |
|<br>
| bgcolor="EEFFFF" |
|[[Atomic Layer Deposition Recipes#AlN deposition .28ALD CHAMBER 3.29|R3]]
| bgcolor="EEFFFF" |
|<br>
| bgcolor="EEFFFF" |
| bgcolor="EEFFFF" |
| bgcolor="EEFFFF" |
|-
|-
!Hg
! bgcolor="#D0E7FF" align="center" | Pd
|
| {{Al/E1}}
|
| <br>
|
| {{Al/E3}}
|
| {{Al/E4}}
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
| <br>
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Pt
! bgcolor="#d0e7ff" align="center" |In
| bgcolor="EEFFFF" | {{Al/E1}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{Al/E3}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{Al/E4}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | [[Sputtering Recipes|A]]
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | [[Sputtering Recipes|R]]
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R3]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Ru
! bgcolor="#d0e7ff" align="center" |Ir
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
| {{Al/E1}}
| <br>
|<br>
| <br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R1]]
| {{Al/E4}}
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
|
| <br>
|
| <br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
|<br>
| <br>
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Si
! bgcolor="#d0e7ff" align="center" |ITO
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{Al/E2}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R4]]
| bgcolor="EEFFFF" | {{Al/E3}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |R1
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |R1
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{rl|PECVD Recipes|amorphous-Si deposition (PECVD-2)}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{rl|PECVD Recipes|amorphous-Si deposition (Unaxis VLR)}}
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
!KCl
! bgcolor="#D0E7FF" align="center" | SiN
|
| {{Al/E1}}
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| {{rl|Sputtering Recipes|SiN deposition (Sputter 3)}}
|
| [[Sputtering Recipes|A]]
|
| <br>
|
| {{rl|Sputtering Recipes|SiN deposition (IBD)}}
|
| <br>
|
| <br>
|
| {{rl|PECVD Recipes|SiN deposition (PECVD #1)}}
|
| {{rl|PECVD Recipes|SiN deposition (PECVD #2)}}
|
| {{rl|PECVD Recipes|SiN deposition (Unaxis VLR)}}
| <br>
| <br>
|-
|-
!LiF
! bgcolor="#D0E7FF" align="center" | SiO<sub>2</sub>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | {{Al/E2}}
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | {{rl|Sputtering Recipes|SiO2 deposition (Sputter 3)}}
|
| bgcolor="EEFFFF" | [[Sputtering Recipes|A]]
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | {{rl|Sputtering Recipes|SiO2 deposition (IBD)}}
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | {{rl|PECVD Recipes|SiO2 deposition (PECVD #1)}}
|
| bgcolor="EEFFFF" | {{rl|PECVD Recipes|SiO2 deposition (PECVD #2)}}
|
| bgcolor="EEFFFF" | {{rl|PECVD Recipes|SiO2 deposition (Unaxis VLR)}}
| bgcolor="EEFFFF" | {{rl|Atomic Layer Deposition Recipes|SiO2 deposition (ALD)}}
| bgcolor="EEFFFF" | <br>
|-
|-
!Mg
! bgcolor="#D0E7FF" align="center" | SiO<sub>x</sub>N<sub>y</sub>
|
| <br>
|
| {{Al/E2}}
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
| <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
| [[Ion_Beam_Deposition_(Veeco_NEXUS)|R]]
|
| <br>
|
| <br>
|
| [[PECVD_Recipes#PECVD_1_.28PlasmaTherm_790.29|R]]
|
| <br>
|
| <br>
| <br>
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Sn
! bgcolor="#d0e7ff" align="center" |MgF2
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
|[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | SrF<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |MgO
|
| <br>
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
| {{Al/E2}}
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
| <br>
| <br>
|-
|-
!Mn
! bgcolor="#D0E7FF" align="center" | Ta
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | {{rl|Sputtering Recipes|Ta deposition (Sputter 3)}}
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
!MnS
! bgcolor="#D0E7FF" align="center" | Ta<sub>2</sub>O<sub>5</sub>
|
| <br>
|
| <br>
|
| <br>
|
| {{Al/E2}}
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| {{rl|Sputtering Recipes|Ta2O5 deposition (IBD)}}
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
| <br>
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Ti
! bgcolor="#d0e7ff" align="center" |Mo
| bgcolor="EEFFFF" | {{Al/E1}}
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{Al/E3}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{Al/E4}}
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | [[Sputtering Recipes|A]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | {{rl|Sputtering Recipes|Ti-Au Deposition (Sputter 4)}}
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="#eeffff" |<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
!Na
! bgcolor="#D0E7FF" align="center" | TiN
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| [[Sputtering Recipes|R]]
|
| <br>
|
| [[Ion_Beam_Deposition_(Veeco_NEXUS)|A]]
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
| <br>
| <br>
|-
|-
!NaCl
! bgcolor="#D0E7FF" align="center" | TiW
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | {{rl|Sputtering Recipes|W-TiW Deposition (Sputter 4)}}
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | TiO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |Nb
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | {{Al/E2}}
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | {{Rl|Sputtering Recipes|TiO2 deposition (Sputter 2)}}
|[[Sputtering Recipes|R3]]
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | {{Rl|Sputtering Recipes|TiO2 deposition (IBD)}}
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | {{rl|Atomic Layer Deposition Recipes|TiO2 deposition (ALD)}}
| bgcolor="EEFFFF" | <br>
|-
|-
!NbO5
! bgcolor="#D0E7FF" align="center" | V
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
|
| <br>
| <br>
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | W
! bgcolor="#d0e7ff" align="center" |Nd
|
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | {{rl|Sputtering Recipes|W deposition (Sputter 4)}}
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Zn
! bgcolor="#d0e7ff" align="center" |Ni
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R6]]
| <br>
| <br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| <br>
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Ni|R6]]
| <br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| <br>
| <br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |R1
| <br>
| <br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
| <br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
| <br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| bgcolor="#eeffff" |<br>
| <br>
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | ZnO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |NiCr
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
|
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | Zr
! bgcolor="#d0e7ff" align="center" |NiFe
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
| <br>
| bgcolor="#eeffff" |
| <br>
| bgcolor="#eeffff" |
| <br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| {{Al/E4}}
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| <br>
| bgcolor="#eeffff" |
| <br>
| bgcolor="#eeffff" |
| <br>
| bgcolor="#eeffff" |
| <br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
| <br>
| bgcolor="#eeffff" |
| <br>
| bgcolor="#eeffff" |
| <br>
| bgcolor="#eeffff" |
| <br>
| bgcolor="#eeffff" |
| <br>
| bgcolor="#eeffff" |
| <br>
| bgcolor="#eeffff" |
| <br>
| <br>
| <br>
|-
|-
! bgcolor="#D0E7FF" align="center" | ZrO<sub>2</sub>
! bgcolor="#d0e7ff" align="center" |Pd
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="EEFFFF" | <br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| bgcolor="EEFFFF" | <br>
|[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
|[[Sputtering Recipes|R1]]
| bgcolor="EEFFFF" | <br>
|R1
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
| bgcolor="EEFFFF" | <br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
|<br>
| bgcolor="EEFFFF" | <br>
| bgcolor="EEFFFF" | {{rl|Atomic Layer Deposition Recipes|ZrO2 deposition (ALD)}}
| bgcolor="EEFFFF" | <br>
|-
|-
! width="20" bgcolor="#D0E7FF" align="center" | '''Material'''
! bgcolor="#d0e7ff" align="center" |Pt
| width="65" bgcolor="#DAF1FF" | [[E-Beam Evaporation Recipes#E-Beam_1_.28Sharon.29|E-Beam 1 (Sharon)]]
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| width="65" bgcolor="#DAF1FF" | [[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]]
| width="65" bgcolor="#DAF1FF" | [[E-Beam Evaporation Recipes#E-Beam_3_.28Temescal.29|E-Beam 3 (Temescal)]]
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| width="65" bgcolor="#DAF1FF" | [[E-Beam Evaporation Recipes#E-Beam_4_.28CHA.29|E-Beam 4 (CHA)]]
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
| width="65" bgcolor="#DAF1FF" | [[Sputtering Recipes#Sputter_1_.28Custom.29|Sputter 1 (Custom)]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| width="65" bgcolor="#DAF1FF" | [[Sputtering Recipes#Sputter_2_.28SFI_Endeavor.29|Sputter 2<br>(SFI Endeavor)]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| width="65" bgcolor="#DAF1FF" | [[Sputtering Recipes#Sputter_3_.28ATC_2000-F.29|Sputter 3<br>(ATC 2000-F)]]
| bcolor="EEFFFF" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |<br>
| width="65" bgcolor="#DAF1FF" | [[Sputtering Recipes#Sputter_4_.28ATC_2200-V.29|Sputter 4<br>(ATC 2200-V)]]
| bgcolor="#eeffff" |<br>
| width="65" bgcolor="#DAF1FF" | [[Sputtering Recipes#Sputter_5_.28Lesker_AXXIS.29|Sputter 5 (Lesker AXXIS)]]
| bgcolor="#eeffff" |
| width="55" bgcolor="#DAF1FF" | [[Ion Beam Deposition (Veeco NEXUS)|Ion Beam<br>Deposition (Tool)]]
| bgcolor="#eeffff" |<br>
| width="45" bgcolor="#DAF1FF" | [[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]]
| bgcolor="#eeffff" |<br>
| width="65" bgcolor="#DAF1FF" | [[Thermal Evaporation Recipes#Thermal_Evap_2_.28Solder.29|Thermal Evap 2 (Solder)]]
| bgcolor="#eeffff" |<br>
| width="65" bgcolor="#DAF1FF" | [[PECVD Recipes#PECVD_1_.28PlasmaTherm_790.29|PECVD 1<br>(PlasmaTherm 790)]]
| width="65" bgcolor="#DAF1FF" | [[PECVD Recipes#PECVD_2_.28Advanced_Vacuum.29|PECVD 2<br>(Advanced Vacuum)]]
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]]
| bgcolor="#eeffff" |<br>
| width="65" bgcolor="#DAF1FF" | [[PECVD Recipes#Unaxis_VLR_ICP-PECVD|Unaxis VLR ICP-PECVD]]
|-
| width="65" bgcolor="#DAF1FF" | [[Atomic Layer Deposition (Oxford FlexAL)|Atomic Layer Deposition (Tool)]]
! bgcolor="#d0e7ff" align="center" |Ru
| width="65" bgcolor="#DAF1FF" | [[Molecular Vapor Deposition|Molecular Vapor Deposition (Tool)]]
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
|<br>
|[[Sputtering Recipes#Ru Deposition .28Sputter 4.29|R3]]
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]]
|<br>
|-
! bgcolor="#d0e7ff" align="center" |Si
| bgcolor="#eeffff" |<br>R1
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[https://wiki.nanotech.ucsb.edu/w/index.php?title=PECVD_Recipes#Amorphous-Si_deposition_.28PECVD_.232.29 R3]
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
! bgcolor="#d0e7ff" align="center" |SiN
|<br>
|<br>
|<br>
|<br>
|[[Sputtering Recipes|R3]]
|[[Sputtering Recipes|R1]]
|<br>
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]]
|<br>
|<br>
|[[PECVD Recipes#SiN deposition .28PECVD .231.29|R6]]
|[[PECVD Recipes#SiN deposition .28PECVD .232.29|R6]]
|[[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|R6]]
|<br>
|<br>
|-
! bgcolor="#d0e7ff" align="center" |SiN - Low Stress
|
|
|
|
|
|
|
|
|
|
|[[PECVD Recipes#Low Stress Si3N4 .28PECVD.231.29|R3]]
|[[PECVD Recipes#Low-Stress SiN deposition .28PECVD .232.29|R6]]
|[[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|R6]]
|
|
|-
!SiN - Low Stress 3xTime
|
|
|
|
|
|
|
|
|
|
|
|[[PECVD Recipes#Low-Stress SiN 3xTime (PECVD #2)|R6]]
|
|
|
|-
! bgcolor="#d0e7ff" align="center" |SiO<sub>2</sub>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R2]]
| bgcolor="#eeffff" |[[Sputtering_Recipes#SiO2_deposition_.28IBD.29|R6]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R6]]
| bgcolor="#eeffff" |[[PECVD Recipes#SiO2 deposition .28PECVD .232.29|R6]]
| bgcolor="#eeffff" |[[PECVD Recipes#ICP-PECVD .28Unaxis VLR.29|R6]]
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]]
| bgcolor="#eeffff" |<br>
|-
!SiO
|
|
|
|
|
|
|
|
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
|
|
|
|
|
|-
! bgcolor="#d0e7ff" align="center" |SiO<sub>x</sub>N<sub>y</sub>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R3]]
|<br>
|<br>
|[[PECVD Recipes#SiO2 deposition .28PECVD .231.29|R3]]
|<br>
|<br>
|<br>
|<br>
|-
! bgcolor="#d0e7ff" align="center" |Sn
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
! bgcolor="#d0e7ff" align="center" |SrF<sub>2</sub>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R1]]
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|-
! bgcolor="#d0e7ff" align="center" |Ta
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
! bgcolor="#d0e7ff" align="center" |Ta<sub>2</sub>O<sub>5</sub>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R1]]
|<br>
|
|<br>
|<br>
|<br>
|[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R6]]
|<br>
|
|<br>
|<br>
|<br>
|<br>
|<br>
|-
! bgcolor="#d0e7ff" align="center" |Ti
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R6]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 3 .28Temescal.29|R2]]
| bgcolor="#eeffff" |[[Process Group - Process Control Data#E-Beam 4: Ti|R6]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R6]]
| bgcolor="#eeffff" |R1
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
! bgcolor="#d0e7ff" align="center" |TiN
|<br>
|<br>
|<br>
|<br>
|<br>
|[[Sputtering Recipes#Sputter 4 (AJA ATC 2200-V)|R3]]
|<br>
|R1
|<br>
|<br>
|<br>
|<br>
|<br>
|[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]]
|<br>
|-
! bgcolor="#d0e7ff" align="center" |TiW
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R1]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes#TiW Co-Sputter Deposition (Sputter 3)|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
! bgcolor="#d0e7ff" align="center" |TiO<sub>2</sub>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 2 .28Custom.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes|R1]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Sputtering Recipes#Si3N4 deposition .28IBD.29|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]]
| bgcolor="#eeffff" |<br>
|-
! bgcolor="#d0e7ff" align="center" |V
|<br>R1
|<br>
|<br>
|<br>R1
|[[Sputtering Recipes|R1]]
|[[Sputtering Recipes|R1]]
|<br>
|<br>
|<br>
|
|<br>
|<br>
|<br>
|<br>
|<br>
|-
! bgcolor="#d0e7ff" align="center" |W
| bgcolor="#eeffff" |[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |R1<br>
| bgcolor="#eeffff" |[[Sputtering Recipes#TiW Co-Sputter Deposition (Sputter 3)|R3]]
| bgcolor="#eeffff" |[[Sputtering Recipes|R3]]
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
|-
!WC
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|
|-
! bgcolor="#d0e7ff" align="center" |Zn
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|<br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 1|R3]]
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R2]]
|<br>
|<br>
|<br>
|<br>
|<br>
|-
! bgcolor="#d0e7ff" align="center" |ZnO
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]]
| bgcolor="#eeffff" |<br>
|-
! bgcolor="#d0e7ff" align="center" |Zr
|[[E-Beam Evaporation Recipes#E-Beam 1 .28Sharon.29|R2]]
|<br>
|<br>
|[[E-Beam Evaporation Recipes#E-Beam 4 .28CHA.29|R2]]
|[[Sputtering Recipes|R1]]
|[[Sputtering Recipes|R1]]
|<br>
|<br>
|<br>
|[[Thermal Evaporation Recipes#Thermal Evaporator 2|R1]]
|<br>
|<br>
|<br>
|<br>
|<br>
|-
! bgcolor="#d0e7ff" align="center" |ZrO<sub>2</sub>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |<br>
| bgcolor="#eeffff" |[[Atomic Layer Deposition Recipes#Pt deposition .28ALD CHAMBER 1.29|R3]]
| bgcolor="#eeffff" |<br>
|-
! width="20" bgcolor="#d0e7ff" align="center" |'''Material'''
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_1_.28Sharon.29|E-Beam 1 (Sharon)]]
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_2_.28Custom.29|E-Beam 2 (Custom)]]
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_3_.28Temescal.29|E-Beam 3 (Temescal)]]
| width="65" bgcolor="#daf1ff" |[[E-Beam Evaporation Recipes#E-Beam_4_.28CHA.29|E-Beam 4 (CHA)]]
| width="65" bgcolor="#daf1ff" |[[Sputtering Recipes#Sputter_3_.28ATC_2000-F.29|Sputter 3<br>(ATC 2000-F)]]
| width="65" bgcolor="#daf1ff" |[[Sputtering_Recipes#Sputter_4_.28AJA_ATC_2200-V.29|Sputter 4<br>(ATC 2200-V)]]
| width="65" bgcolor="#daf1ff" |[[Sputtering Recipes|Sputter 5 (ATC 2200-V)]]
| width="55" bgcolor="#daf1ff" |[[Sputtering_Recipes#Ion_Beam_Deposition_.28Veeco_NEXUS.29|Ion Beam<br>Deposition (Veeco Nexus)]]
| width="45" bgcolor="#daf1ff" |[[Thermal Evaporation Recipes#Thermal_Evap_1|Thermal<br>Evap 1]]
| width="65" bgcolor="#daf1ff" |[[Thermal Evaporation Recipes#Thermal_Evap_2_.28Solder.29|Thermal Evap 2 (Solder)]]
| width="65" bgcolor="#daf1ff" |[[PECVD Recipes#PECVD_1_.28PlasmaTherm_790.29|PECVD 1<br>(PlasmaTherm 790)]]
| width="65" bgcolor="#daf1ff" |[[PECVD Recipes#PECVD_2_.28Advanced_Vacuum.29|PECVD 2<br>(Advanced Vacuum)]]
| width="65" bgcolor="#daf1ff" |[[PECVD_Recipes#ICP-PECVD_.28Unaxis_VLR.29|Unaxis VLR ICP-PECVD]]
| width="65" bgcolor="#daf1ff" |[[Atomic_Layer_Deposition_Recipes|Atomic Layer Deposition (Oxford FlexAl)]]
| width="65" bgcolor="#daf1ff" |[[Molecular Vapor Deposition|Molecular Vapor Deposition (Tool)]]
|}
|}


===Process Ranking Table===
Processes in the table above are ranked by their "''Process Maturity Level''" as follows:
{| class="wikitable"
!Process Level
! colspan="11" |Description of Process Level Ranking
|-
|A
| colspan="11" |Process '''A'''llowed and materials available but never done
|-
|R1
| colspan="11" |Process has been ran at least once
|-
|R2
| colspan="11" |Process has been ran and procedure is documented
|-
|R3
| colspan="11" |Process has been ran, procedure is documented, and data is available
|-
|R4
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''no''' in-Situ control available
|-
|R5
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' in-Situ control available
|-
|R6
| colspan="11" |Process has a documented procedure and control charts/limits available.  Controlled process.
|}
[[Category:Processing]]
[[Category:Processing]]

Latest revision as of 06:38, 23 January 2026

Process Control Data

See linked page for process control data (calibration data over time, such as dep. rate, refractive index, stress etc.) over time, for a selection of highly used tools/films.

Deposition Tools/Materials Table

Process Maturity Ranking

  • R6 - most mature process with regular calibrations recorded on SPC charts.
  • …
  • R1 - least mature - "possible" but you'll have to figure it out.

The Key/Legend for this table's R1...R6 values is at the bottom of the page.

Vacuum Deposition Recipes

E-Beam Evaporation Sputtering Thermal Evaporation Plasma Enhanced Chemical
Vapor Deposition (PECVD)
Atomic Layer Deposition Molecular Vapor Deposition
Material E-Beam 1 (Sharon) E-Beam 2 (Custom) E-Beam 3 (Temescal) E-Beam 4 (CHA) Sputter 3
(AJA ATC 2000-F)
Sputter 4
(AJA ATC 2200-V)
Sputter 5 (AJA ATC 2200-V) Ion Beam
Deposition (Veeco Nexus)
Thermal
Evap 1
Thermal Evap 2 (Solder) PECVD 1
(PlasmaTherm 790)
PECVD 2
(Advanced Vacuum)
Unaxis VLR ICP-PECVD Atomic Layer Deposition (Oxford FlexAL) Molecular Vapor Deposition (Tool)
Ag R2
R2 R2 R1 R1
R1 R1




AgBr
AgCl
Al R2
R2 R2 R1 R3 R6 R1 R3 R1




Al2O3 R2

R3 R3 R1 R3




R3
AuPd R1 R1 R1
AuZn R1
AuSn R1
AuGe R2 R1 R2
AlN



R1 R1
R1




R3
Au R6
R2 R6 R1 R2 R3
R3 R2




B













C R3
CaF2 R2
CeO2
R3












Co R2

R2 R3


R1 R1




Cr R6
R2
R6 R3
R6
R3 R2




Cu R1


R3 R2

R2 R1




Fe R2

R2 R3


R1 R1




Ge R2
R2
R2 R2 R1 R1







GeO2 R1
Gd R2

R1










Hf R1


R1











HfO2



R1





R3
Hg
In








R3




Ir R1

R1








ITO
R4

R1 R1 R1 R1






KCl
LiF
Mg R1 R1
MgF2 R1 R1 R1
MgO R2
Mn
MnS
Mo R2


R3 R1






Na
NaCl
Nb R2



R3






NbO5
Nd



R1






Ni R6
R2 R6 R3
R1
R3 R2




NiCr R2 R2 R3
NiFe R1 R2 R1 R3
Pd R2
R2 R2 R1 R1 R1
R3 R1




Pt R2
R2 R2 R3 R3 R3




R3
Ru R2

R2
R3






R3
Si
R1
R2

R3 R1
R1

R3

SiN



R3 R1
R6

R6 R6 R6

SiN - Low Stress R3 R6 R6
SiN - Low Stress 3xTime R6
SiO2 R2 R2

R3 R1 R2 R6
R6 R6 R6 R3
SiO R1 R1
SiOxNy






R3

R3



Sn








R2




SrF2
R2





R1





Ta R1


R3 R1
R1





Ta2O5
R1



R6





Ti R6
R2 R6 R3 R3 R6 R1





TiN




R3
R1




R3
TiW R1


R3 R3








TiO2
R2

R1 R3
R3



R3
V
R1



R1
R1 R1







W R2

R1
R3 R3







WC
Zn







R3 R2




ZnO










R3
Zr R2

R2 R1 R1


R1




ZrO2











R3
Material E-Beam 1 (Sharon) E-Beam 2 (Custom) E-Beam 3 (Temescal) E-Beam 4 (CHA) Sputter 3
(ATC 2000-F)
Sputter 4
(ATC 2200-V)
Sputter 5 (ATC 2200-V) Ion Beam
Deposition (Veeco Nexus)
Thermal
Evap 1
Thermal Evap 2 (Solder) PECVD 1
(PlasmaTherm 790)
PECVD 2
(Advanced Vacuum)
Unaxis VLR ICP-PECVD Atomic Layer Deposition (Oxford FlexAl) Molecular Vapor Deposition (Tool)

Process Ranking Table

Processes in the table above are ranked by their "Process Maturity Level" as follows:

Process Level Description of Process Level Ranking
A Process Allowed and materials available but never done
R1 Process has been ran at least once
R2 Process has been ran and procedure is documented
R3 Process has been ran, procedure is documented, and data is available
R4 Process has a documented procedure with regular (≥4x per year) data no in-Situ control available
R5 Process has a documented procedure with regular (≥4x per year) data and in-Situ control available
R6 Process has a documented procedure and control charts/limits available.  Controlled process.