PECVD Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
→SiO2 deposition (PECVD #2): mentioned RIX, stress etc.
Biljana (talk | contribs)
→Si3N4 [ICP-PECVD]: SiN parameters
 
(30 intermediate revisions by 2 users not shown)
Line 38: Line 38:


==Standard Cleaning Procedure (PECVD #1)==
==Standard Cleaning Procedure (PECVD #1)==
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully.


The clean is done in two steps:
⚫
#Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )

⚫
#Load the recipe for cleaning "CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding a required time for cleaning.
⚫
#'''Wet cleaning''' (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
#
⚫
#Load the recipe for plasma cleaning "'''''CF4/O2 Clean'''''" (run the recipe and it will pop-up asking for the cleaning time). Follow instructions regarding a required time for cleaning.


{| class="wikitable"
{| class="wikitable"
Line 50: Line 51:
|-
|-
|SiO<sub>2</sub>
|SiO<sub>2</sub>
|1 min clean for every 1 min dep
|TBD
|-
|-
|Si<sub>3</sub>N<sub>4</sub>
|Si<sub>3</sub>N<sub>4</sub>
|1 min clean for every 7 min dep
|TBD
|-
|-
|SiOxNy
|SiOxNy
|Same as XYZ
|Same as SiO<sub>2</sub>
|-
|a-Si
|Same time as Si<sub>3</sub>N<sub>4</sub>
|}
|}

#


===[https://wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"]===
===[https://wiki.nanotech.ucsb.edu/w/images/7/72/PECVD1-cleaning.png Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"]===
Line 110: Line 112:
==Amorphous-Si deposition (PECVD #2)==
==Amorphous-Si deposition (PECVD #2)==


*[[PECVD-2 - a-Si Recipe and Dep process (2025)|a-Si Recipe and Dep process]] 2025-11
⚫
*[https://wiki.nanotech.ucsb.edu/wiki/images/9/9d/03-Amorphous-Si-PECVD-2.pdf Amorphous Si Deposition Recipe]
**''Developed by Ryan Hersey & Skyler Palatnik, Group of Prof. Max Millar-Blanchaer''
⚫
*[https://wiki.nanotech.ucsb.edu/wiki/images/0/09/ASi_deposition_and_film_stress_using_AV_dep_tool.pdf Amorphous Si Film Characterization and Stress]
⚫
*[https://wiki.nanotech.ucsb.edu/wiki/images/9/9d/03-Amorphous-Si-PECVD-2.pdf Amorphous Si Deposition Recipe] (2013-09, Ning Cao)
⚫
*[https://wiki.nanotech.ucsb.edu/wiki/images/0/09/ASi_deposition_and_film_stress_using_AV_dep_tool.pdf Amorphous Si Film - Characterization and Stress] - DOE/recipe variations


==Standard Cleaning Procedure (PECVD #2)==
==Standard Cleaning Procedure (PECVD #2)==
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:
The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:


#(If >29min dep time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again.
#If > 29min (season+dep. time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again. Do not clean shower-head!
#Load the recipe for cleaning "STD CF<sub>4</sub>/O<sub>2</sub> Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.
#Load the recipe for cleaning "STD CF<sub>4</sub>/O<sub>2</sub> Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.


===[https://wiki.nanotech.ucsb.edu/w/images/3/34/PECVD2_photo_for_cleaning.png Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"]===
===[https://wiki.nanofab.ucsb.edu/wiki/File:STD_CF4-O2_Clean_PECVD2.jpg Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"]===
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.
Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.


Line 129: Line 133:
|-
|-
|SiO<sub>2</sub>
|SiO<sub>2</sub>
|1 min. clean for every 1 min. deposition
|1min. clean for every 1min. deposition
|-
|-
|Si<sub>3</sub>N<sub>4</sub>
|Si<sub>3</sub>N<sub>4</sub>
|1 min. clean for every 7 min of deposition
|1min. clean for every 7min. of deposition
|-
|-
|a-Si
|2 min clean for every 1min of deposition
|-
|a-Si (max 60min dep before breaking it up and cleaning the chamber)
⚫
|Wet Clean the Upper Lid/Chamber
DI water then Isopropyl Alcohol on chamber wall & portholes
|-
|Other films:(max 60min long dep. in one single run)
|If > 29min total dep time
|If > 29min total dep time
(Season + Dep)
(Season + Dep)

⚫
|Wet Clean the Upper Lid/Chamber
Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes
DI water then Isopropyl Alcohol on chamber wall & portholes
|}
|}
Line 193: Line 207:
==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==
==Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==


*[https://docs.google.com/spreadsheets/d/18nE-iTLLH4QIq3wadHVgjVuZ215o9xUz_aCX2WDdges/edit?gid=638997025#gid=638997025 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN 250C-new May 2024''"
* [https://docs.google.com/spreadsheets/d/1xvXqgFaKT6vH4ZSAfOaqAYnx_qyEqzNZFqTc-OGENzw/edit?gid=1168016715#gid=1168016715 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD]- Standard Recipe</nowiki>] - ''"SiN 250C-v2- New recipe since April 2026"''
**recipe "SiN 250C-v2", sequence "SiN 250C-v2", category "SiN Std."
**this film has a low particle count (good for waveguides)
**requires 30sec O2 plasma using PE-II beforehand
**dep.rate=90.86nm/min, refractive index at 632.8nm=2.04372, refractive index at 1550nm=2.00804, stress=-183MPa
**Cauchy A=2.004+/-0.0013, B=0.00745+/-0.00072928, C=0.00999+/-0.00011018


* [https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1670372499 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
* *[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit?gid=1670372499#gid=1670372499 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
** Lists film data, such as dep rate, stress, particle count, refractive index etc.
** Lists film data, such as dep rate, stress, particle count, refractive index etc.


Line 203: Line 222:
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Old Recipe] - 2019
*[https://docs.google.com/spreadsheets/d/1VrgS0cB2OcdZVTCnDAesgQCLRaAgEB_Iajc_OrhXOo0/edit#gid=1199123007 Old Recipe] - 2019
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_250C_deposition_.28Unaxis_VLR.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021
*[https://wiki.nanotech.ucsb.edu/wiki/Old_Deposition_Data_-_2021-12-15#SiN_250C_deposition_.28Unaxis_VLR.29 Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Historical Data</nowiki>] - before Oct. 2021

** Lists film data, such as dep rate, stress, particle count, refractive index etc.


==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==
==Low Stress Si<sub>3</sub>N<sub>4</sub> [ICP-PECVD]==


*[https://docs.google.com/spreadsheets/d/1xchMuXlPABSKcW-rMau8B-cw_jnJnwI9qpXqDLUQ8sU/edit?gid=1239658204#gid=1239658204 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C-new May 2024''"
*[https://docs.google.com/spreadsheets/d/1xchMuXlPABSKcW-rMau8B-cw_jnJnwI9qpXqDLUQ8sU/edit?gid=1239658204#gid=1239658204 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Standard Recipe</nowiki>] - "''SiN Low Stress 250C-new May 2024''"
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
*[https://docs.google.com/spreadsheets/d/1CuDMKFTTzGLL6CP-FEI_9cOnUaIw-432ppDFssB59wY/edit#gid=1517031044 Low Stress Si<sub>3</sub>N<sub>4</sub><nowiki> [ICP-PECVD] - Current Process Control Data</nowiki>]
**Lists film data, such as dep rate, stress, particle count, refractive index etc.
**Lists film data, such as dep rate, stress, particle count, refractive index etc.

Latest revision as of 21:34, 28 September 2026

Back to Vacuum Deposition Recipes.

PECVD 1 (PlasmaTherm 790)

PECVD 1 Process Control Plots - Plots of all process control data

SiO2 deposition (PECVD #1)

Old Data

SiN deposition (PECVD #1)

Old Data

Low Stress Si3N4 (PECVD#1)

plot of SiN stress and Refractive Index vs. N2 flow.
Example of Si3N4 modified stress via. varying N2 flow.  Refractive index is relatively constant (one outlier), and stress varies continuously from tensile to compressive.  (Demis D. John 2011, Blumenthal Group)

SiOxNy deposition (PECVD #1)

Standard Cleaning Procedure (PECVD #1)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully.

The clean is done in two steps:

  1. Wet cleaning (start cleaning by using a cleanroom wipe sprayed with DI. Wipe chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA. )
  2. Load the recipe for plasma cleaning "CF4/O2 Clean" (run the recipe and it will pop-up asking for the cleaning time). Follow instructions regarding a required time for cleaning.
Table of Cleaning Times
Film Dep'd Cleaning Time
SiO2 1 min clean for every 1 min dep
Si3N4 1 min clean for every 7 min dep
SiOxNy Same as SiO2
a-Si Same time as Si3N4

Standard Cleaning Recipe (PECVD#1): "CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.

PECVD 2 (Advanced Vacuum)

PECVD 2 Process Control Plots - Plots of all process control data

SiO2 deposition (PECVD #2)

  • SiO2 deposition rate at 150C is 35nm/min

SiN deposition (PECVD #2)

Low-Stress SiN deposition (PECVD #2)

Low-Stress Silicon Nitride, Si3N4 (< ±100 MPa)

Low-Stress SiN 3xTime (PECVD #2)

This Low-Stress SiN recipe is more stable over time (months), because each step is 3x longer (so each compressive/tensile layer is thicker), making it less susceptible to RF ignition delays as the grounding strap is etched over time. – 2024-09 Demis & Biljana

Amorphous-Si deposition (PECVD #2)

Standard Cleaning Procedure (PECVD #2)

The cleaning procedure is very important in order to have consistent result on this tool and also to keep particulate count low. After each deposition you should clean the tool following instructions carefully. The clean is done in two steps:

  1. If > 29min (season+dep. time) Wet cleaning: Start cleaning by using a cleanroom wipe sprayed with DI. Wipe upper chamber sidewalls with it. Finish cleaning by using the cleanroom wipe sprayed with IPA & wiping again. Do not clean shower-head!
  2. Load the recipe for cleaning "STD CF4/O2 Clean" (edit the recipe and change ONLY time of cleaning). Follow instructions regarding required time for cleaning.

Standard Clean Recipe (PECVD#2): "STD CF4/O2 Clean"

Click the above link for a screenshot of the standard cleaning recipe, for which you will enter a custom time. The recipe is set up so that it will pop up a window for the cleaning time upon running the recipe - you do not need to edit the recipe before running it.


Clean Times (PECVD#2)

Film Deposited Cleaning Time (Dry)
SiO2 1min. clean for every 1min. deposition
Si3N4 1min. clean for every 7min. of deposition
a-Si 2 min clean for every 1min of deposition
a-Si (max 60min dep before breaking it up and cleaning the chamber) Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes

Other films:(max 60min long dep. in one single run) If > 29min total dep time

(Season + Dep)

Wet Clean the Upper Lid/Chamber

DI water then Isopropyl Alcohol on chamber wall & portholes

ICP-PECVD (Unaxis VLR)

2020-02: New recipes have been characterized for low particulate count and repeatability.  Only staff-supplied recipes are allowed in the tool. Please follow the new procedures to ensure low particle counts in the chamber.
The system currently has Deuterated Silane (SiD4) installed - identical to the regular Silicon precursor SiH4, except that it significantly lowers optical absorption in the near-infrared due to shifted molecular vibrations/molecular weights. This gas is more expensive and thus more applicable to optical application than to general-purpose SiN films.

Process Control Data (Unaxis ICP-PECVD)

Regularly-run depositions and measurements of film properties over time - executed by NanoFab Interns.

Low Deposition Rate SiO2 [ICP-PECVD]

Old Data

High Deposition Rate SiO2 [ICP-PECVD]

Old Data

Gap-Fill SiO2 [ICP-PECVD]

Recipe designed by Warren Jin, please consider our publication policy if you publish using this recipe.

NOTE: Please contact tool supervisor before running this recipe - this recipe must often be scheduled to prevent excessive chamber maintenance.

Able to effectively fill ~1:1 and ~1:2 aspect ratio gaps in Silicon and Glass structures (eg. waveguides/optical gratings) with void-free filling.

The recipe uses a high 400W RF Bias to reduce buildup on corners that causes voids during growth.

  • Category = SiO2 GapFill - Std.
  • FLOW: SiO2 GapFill 250C
    • Will run the sequence SiO2 GapFill 250C 450W. Do not change this!
  • STEP (edit TIME only): SiO2 GapFill 250C
  • Deposition rate = 99.968nm/min [9/20/23]

Si3N4 [ICP-PECVD]

  • Si3N4 [ICP-PECVD]- Standard Recipe - "SiN 250C-v2- New recipe since April 2026"
    • recipe "SiN 250C-v2", sequence "SiN 250C-v2", category "SiN Std."
    • this film has a low particle count (good for waveguides)
    • requires 30sec O2 plasma using PE-II beforehand
    • dep.rate=90.86nm/min, refractive index at 632.8nm=2.04372, refractive index at 1550nm=2.00804, stress=-183MPa
    • Cauchy A=2.004+/-0.0013, B=0.00745+/-0.00072928, C=0.00999+/-0.00011018

Old Data

    • Lists film data, such as dep rate, stress, particle count, refractive index etc.

Low Stress Si3N4 [ICP-PECVD]

Old Data

Standard Seasoning Procedure [ICP-PECVD]

You must edit the seasoning recipes (SiO2 Seasoning - Std, SiN seasoning - Std). You are allowed to change only seasoning time [time needed to coat chamber walls with ~200nm of film]. Seasoning recipes:

Standard Cleaning Procedure [ICP-PECVD]

You must edit the Post-Dep Clean recipe to correspond to your deposited thickness and material. See the Operating Procedure on the Unaxis Tool Page for details.

  • SiNx etches at 20nm/min
  • SiO2 etches at 40nm/min

Standard Clean Recipe

General Recipe Notes (Unaxis VLR ICP-PECVD)

  • RF1 = Bias
  • RF2 = ICP Power
  • All recipes start with an Argon pre-clean with 0W bias (gentle), to improve adhesion/nucleation.
  • Maximum SiO2 Dep. thickness allowed: 800nm