Sputtering Recipes: Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Biljana (talk | contribs)
Biljana (talk | contribs)
Line 54: Line 54:
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dFRJLUZUdXB4WFA1S1BMMWQ4WndpTWc&usp=drive_web#gid=sharing Oxide Data March 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dFRJLUZUdXB4WFA1S1BMMWQ4WndpTWc&usp=drive_web#gid=sharing Oxide Data March 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGNyV083bmpzMjZpZ0JFVWhoOUpaN3c#gid=0=sharing Oxide Thickness uniformity 2014]
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGNyV083bmpzMjZpZ0JFVWhoOUpaN3c#gid=0=sharing Oxide Thickness uniformity 2014]
*IBD SiO{{sub|2}} Typical Film Properties( Deposition rate, Refractive index, Stress)

⚫
* Deposition Rate: ≈5.6 nm/min (users must calibrate this prior to critical deps)
* Refractive Index: ≈1.487
* Refractive Index: ≈1.487
⚫
* Rate: ≈5.6 nm/min (users must calibrate this prior to critical deps)
* Stress ≈ -387MPa (compressive)
* Stress ≈ -387MPa (compressive)



Revision as of 21:20, 1 April 2014

Back to Vacuum Deposition Recipes.

Sputter 1 (Custom)

Sputter 2 (SFI Endeavor)

Al Deposition (Sputter 2)

AlNx Deposition (Sputter 2)

Au Deposition (Sputter 2)

TiO2 Deposition (Sputter 2)

Sputter 3 (AJA ATC 2000-F)

The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended.

Material P(mT) Pow(W) Sub(W) T(C) Ar N2 O2 Height-Tilt Rate(nm/min) Stress(MPa) Rs(uOhm-cm) n@633nm k@633nm Data Below Comment
XXX XXX XXX XXX XXX XXX XXX XXX XXX XXX XXX XXX XXX XXX XXX XXX


Ni and Ta Deposition (Sputter 3)

Sputter 4 (AJA ATC 2200-V)

The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended.

Material P(mT) Pow(W) Sub(W) T(C) Ar N2 O2 Height-Tilt Rate(nm/min) Stress(MPa) Rs(uOhm-cm) n@633nm k@633nm Data Below Comment
W 3 300 0 50 45 0 0 H2.75-T5 11.5 -150 to 150 11 - - Yes Jeremy Watcher
TiW 4.5 300 0 75 45 0 0 H2.75-T5 9.5 -150 to 150 60 - - Yes 10%Ti by Wt

W-TiW Deposition (Sputter 4)

Sputter 5 (Lesker AXXIS)

Ion Beam Deposition (Veeco NEXUS)

IBD Calibrations Spreadsheet - Records of historical film depositions (rates, indices), Uniformity etc.

All users are required to enter their calibration deps (simple test deps only)

SiO2 deposition (IBD)

Si3N4 deposition (IBD)

Ta2O5 deposition (IBD)

  • Refractive Index ≈ 2.10
  • Rate ≈7.8nm/min (users must calibrate this prior to critical deps)
  • Stress ≈ -140MPa (compressive)

TiO2 deposition (IBD)