Sputtering Recipes: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
| Line 95: | Line 95: | ||
==Ta{{sub|2}}O{{sub|5}} deposition (IBD)== |
==Ta{{sub|2}}O{{sub|5}} deposition (IBD)== |
||
*[[media:IBD Ta2O5 deposition details.pdf|Ta{{sub|2}}O{{sub|5}} Standard Recipe]] |
*[[media:IBD Ta2O5 deposition details.pdf|Ta{{sub|2}}O{{sub|5}} Standard Recipe]] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGhhUGdCR2JudkZJU3pBemR4bS1GWWc#gid=0=sharing Ta{{sub|2}}O{{sub|5}} Data |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGhhUGdCR2JudkZJU3pBemR4bS1GWWc#gid=0=sharing Ta{{sub|2}}O{{sub|5}} Data December 2014] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dE5xbVFyUFZqdTdUN0JRSUNvMGFGb2c#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dE5xbVFyUFZqdTdUN0JRSUNvMGFGb2c#gid=sharing Ta{{sub|2}}O{{sub|5}} Thickness uniformity 2014] |
||
Revision as of 23:37, 3 December 2014
Back to Vacuum Deposition Recipes.
Sputter 1 (Custom)
Sputter 2 (SFI Endeavor)
Al Deposition (Sputter 2)
AlNx Deposition (Sputter 2)
Au Deposition (Sputter 2)
TiO2 Deposition (Sputter 2)
Sputter 3 (AJA ATC 2000-F)
The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended.
| Material | P(mT) | Pow(W) | Sub(W) | T(C) | Ar | N2 | O2 | Height-Tilt | Rate(nm/min) | Stress(MPa) | Rs(uOhm-cm) | n@633nm | k@633nm | Data Below | Comment |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Ni | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 44-4 | 5.23 | - | - | - | - | yes | Ning |
| Ni | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 25-9 | 1.82 | - | - | - | - | yes | Ning |
| Ni | 5 | 75 | 0 | 20 | 25 | 0 | 0 | 44-4 | 2.50 | - | - | - | - | yes | Ning |
| Ta | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 44-4 | 9.47 | - | - | - | - | yes | Ning |
| Ta | 5 | 75 | 0 | 20 | 25 | 0 | 0 | 44-4 | 5.03 | - | - | - | - | yes | Ning |
| SampleClean-NativeSiO2 | 10 | 0 | 18 | 20 | 25 | 0 | 0 | 44-4 | - | - | - | - | - | yes | 150Volts 5 min |
Ni and Ta Deposition (Sputter 3)
Sputter 4 (AJA ATC 2200-V)
The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended.
| Material | P(mT) | Pow(W) | Sub(W) | T(C) | Ar | N2 | O2 | Height-Tilt | Rate(nm/min) | Stress(MPa) | Rs(uOhm-cm) | n@633nm | k@633nm | Data Below | Comment |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| W | 3 | 300 | 0 | 50 | 45 | 0 | 0 | H2.75-T5 | 11.5 | -150 to 150 | 11 | - | - | Yes | Jeremy Watcher |
| TiW | 4.5 | 300 | 0 | 75 | 45 | 0 | 0 | H2.75-T5 | 9.5 | -150 to 150 | 60 | - | - | Yes | 10%Ti by Wt |
| TiN | 4 | 250 | 0 | 250 | 20 | 10 | 0 | H2.00-T7 | 1.9 | - | - | - | - | No | |
| Nb | 4 | 250 | 0 | 20 | 30 | 0 | 0 | H2.00-T7 | 7.5 | - | - | - | - | No |
W-TiW Deposition (Sputter 4)
Sputter 5 (Lesker AXXIS)
Ion Beam Deposition (Veeco NEXUS)
- IBD Calibrations Spreadsheet - Records of historical film depositions (rates, indices), Uniformity etc.
All users are required to enter their calibration deps (simple test deps only)
SiO2 deposition (IBD)
- Deposition Rate: ≈ 5.89 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~489nm/min
- Stress ≈ -410MPa (compressive)
- Refractive Index: ≈ 1.489
- [Cauchy Parameters] (350-2000nm):
- A = 1.480
- B = 0.00498
- C = -3.2606e-5
Si3N4 deposition (IBD)
- Deposition Rate: ≈ 4.13 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~11nm/min
- Stress ≈ -1618MPa (compressive)
- Refractive Index: ≈ 1.970
- [Cauchy Parameters] (350-2000nm):
- A = 2.000
- B = 0.01974
- C = 1.2478e-4
Ta2O5 deposition (IBD)
- Deposition Rate: ≈ 8.18 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~1 nm/min
- Stress ≈ -258MPa (compressive)
- Refractive Index: ≈ 2.172
- [Cauchy Parameters] (350-2000nm):
- A = 2.1123
- B = 0.018901
- C = -0.016222
TiO2 deposition (IBD)
- Deposition Rate: ≈ 1.35 nm/min (users must calibrate this prior to critical deps)
- HF etch rate ~5.48nm/min
- Stress ≈ -422MPa (compressive)
- Refractive Index: ≈ 2.317
- [Cauchy Parameters] (350-2000nm):
- A = 2.435
- B = -4.9045e-4
- C = 0.01309
- Absorbing < ~350nm