Sputtering Recipes: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
| Line 102: | Line 102: | ||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dFRJLUZUdXB4WFA1S1BMMWQ4WndpTWc&usp=drive_web#gid=sharing SiO<sub>2</sub> Data December 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dFRJLUZUdXB4WFA1S1BMMWQ4WndpTWc&usp=drive_web#gid=sharing SiO<sub>2</sub> Data December 2014] |
||
*[https://docs.google.com/spreadsheets/d/1pxQkTm274CVjzlnE3cZgE5ycgXfIk8cVCAwTg5x7Xx4/edit#gid=sharing SiO<sub>2</sub> Data 2015] |
*[https://docs.google.com/spreadsheets/d/1pxQkTm274CVjzlnE3cZgE5ycgXfIk8cVCAwTg5x7Xx4/edit#gid=sharing SiO<sub>2</sub> Data 2015] |
||
*[https://docs.google.com/spreadsheets/d/1qnlny3A8jRUPU-8O1ycx9MUFmpti_pRv93rT1pXHMWM/edit#gid=1868267914=sharing SiO<sub>2</sub> Data-1hr depositions 2015] |
|||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGNyV083bmpzMjZpZ0JFVWhoOUpaN3c#gid=0=sharing SiO<sub>2</sub> Thickness uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dGNyV083bmpzMjZpZ0JFVWhoOUpaN3c#gid=0=sharing SiO<sub>2</sub> Thickness uniformity 2014] |
||
*[https://docs.google.com/spreadsheets/d/1vYSV7iGIMJsqmlxF6bAjdzuaATcDGxBvwlhb2XYJoWg/edit#gid=sharing SiO<sub>2</sub> Thickness uniformity 2015] |
*[https://docs.google.com/spreadsheets/d/1vYSV7iGIMJsqmlxF6bAjdzuaATcDGxBvwlhb2XYJoWg/edit#gid=sharing SiO<sub>2</sub> Thickness uniformity 2015] |
||
Revision as of 21:51, 9 June 2015
Back to Vacuum Deposition Recipes.
Sputter 1 (Custom)
Sputter 2 (SFI Endeavor)
Al Deposition (Sputter 2)
AlNx Deposition (Sputter 2)
Au Deposition (Sputter 2)
TiO2 Deposition (Sputter 2)
Sputter 3 (AJA ATC 2000-F)
The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended.
| Material | P(mT) | Pow(W) | Sub(W) | T(C) | Ar | N2 | O2 | Height-Tilt | Rate(nm/min) | Stress(MPa) | Rs(uOhm-cm) | n@633nm | k@633nm | Data Below | Comment |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| SiO2 | 3 | 200 | 10 | 20 | 25 | 0 | 3 | 25-9 | 3.68 | - | - | 1.447 | - | yes | Brian |
| SiO2 | 3 | 250 | 10 | 20 | 25 | 0 | 2.5 | 25-9 | 4.3 | - | - | 1.485 | - | yes | Brian |
| SiO2 | 3 | 200 | 10 | 20 | 25 | 0 | 5 | 45-3 | 2.60 | - | - | 1.471 | - | yes | Brian |
| SiN | 3 | 200 | 10 | 20 | 25 | 3 | 0 | 25-9 | 1.56 | - | - | 1.992 | - | yes | Brian |
| SiN | 3 | 250 | 10 | 20 | 25 | 2.5 | 0 | 25-9 | 2.1 | - | - | 2.06 | - | yes | Brian |
| Ni | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 44-4 | 5.23 | - | - | - | - | yes | Ning |
| Ni | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 25-9 | 1.82 | - | - | - | - | yes | Ning |
| Ni | 5 | 75 | 0 | 20 | 25 | 0 | 0 | 44-4 | 2.50 | - | - | - | - | yes | Ning |
| Ta | 5 | 150 | 0 | 20 | 25 | 0 | 0 | 44-4 | 9.47 | - | - | - | - | yes | Ning |
| Ta | 5 | 75 | 0 | 20 | 25 | 0 | 0 | 44-4 | 5.03 | - | - | - | - | yes | Ning |
| SampleClean-NativeSiO2 | 10 | 0 | 18 | 20 | 25 | 0 | 0 | 44-4 | - | - | - | - | - | yes | 150Volts 5 min |
Ni and Ta Deposition (Sputter 3)
SiO2 Deposition (Sputter 3)
SiN Deposition (Sputter 3)
Sputter 4 (AJA ATC 2200-V)
The recipes below are given as starting points from data obtained in the nanofab. For critical depositions, calibrations are recommended.
| Material | P(mT) | Pow(W) | Sub(W) | T(C) | Ar | N2 | O2 | Height-Tilt | Rate(nm/min) | Stress(MPa) | Rs(uOhm-cm) | n@633nm | k@633nm | Data Below | Comment |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| W | 3 | 300 | 0 | 50 | 45 | 0 | 0 | H2.75-T5 | 11.5 | -150 to 150 | 11 | - | - | Yes | Jeremy Watcher |
| TiW | 4.5 | 200 | 0 | 20 | 45 | 0 | 0 | H1-T10 | 4.36 | - | - | - | - | No(AFM:available) | Ning Cao |
| TiW | 4.5 | 300 | 0 | 75 | 45 | 0 | 0 | H2.75-T5 | 9.5 | -150 to 150 | 60 | - | - | Yes | 10%Ti by Wt |
| TiN | 4 | 250 | 0 | 250 | 20 | 10 | 0 | H2.00-T7 | 1.9 | - | - | - | - | No | |
| Nb | 4 | 250 | 0 | 20 | 30 | 0 | 0 | H2.00-T7 | 7.5 | - | - | - | - | No | |
| Ti | 10 | 200 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 2.3 | - | - | - | - | Yes | Ning Cao |
| Au | 5 | 200 | 0 | 20 | 45 | 0 | 0 | H1-T10 | 17.7 | - | - | - | - | No(AFM:available) | Ning Cao |
| Au | 10 | 300 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 45.4 | - | - | - | - | Yes | Ning Cao |
| Al | 5 | 200 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 4.4 | - | - | - | - | No(SEM:available | Ning Cao |
| Pt | 5 | 200 | 0 | 20 | 45 | 0 | 0 | H2.75-T5 | 7.32 | - | - | - | - | No(AFM:available) | Ning Cao |
W-TiW Deposition (Sputter 4)
Ti-Au Deposition (Sputter 4)
Sputter 5 (Lesker AXXIS)
Ion Beam Deposition (Veeco NEXUS)
- IBD Calibrations Spreadsheet - Records of historical film depositions (rates, indices), Uniformity etc.
- Particulates in SiO2 and Ta2O5 in 2015
All users are required to enter their calibration deps (simple test deps only)
SiO2 deposition (IBD)
- Deposition Rate: ≈ 5.89 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~489nm/min
- Stress ≈ -410MPa (compressive)
- Refractive Index: ≈ 1.489
- [Cauchy Parameters] (350-2000nm):
- A = 1.480
- B = 0.00498
- C = -3.2606e-5
Si3N4 deposition (IBD)
- Deposition Rate: ≈ 4.10 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~11nm/min
- Stress ≈ -1590MPa (compressive)
- Refractive Index: ≈ 1.969
- [Cauchy Parameters] (350-2000nm):
- A = 2.000
- B = 0.01974
- C = 1.2478e-4
Ta2O5 deposition (IBD)
- Ta2O5 Standard Recipe
- Ta2O5 Data December 2014
- Ta2O5 Data December 2015
- Ta2O5 Thickness uniformity 2014
- Ta2O5 Thickness uniformity 2015
- Deposition Rate: ≈ 8.00 nm/min (users must calibrate this prior to critical deps)
- HF e.r.~1 nm/min
- Stress ≈ -252MPa (compressive)
- Refractive Index: ≈ 2.171
- [Cauchy Parameters] (350-2000nm):
- A = 2.1123
- B = 0.018901
- C = -0.016222
TiO2 deposition (IBD)
- Deposition Rate: ≈ 1.29 nm/min (users must calibrate this prior to critical deps)
- HF etch rate ~5.34nm/min
- Stress ≈ -445MPa (compressive)
- Refractive Index: ≈ 2.259
- [Cauchy Parameters] (350-2000nm):
- A = 2.435
- B = -4.9045e-4
- C = 0.01309
- Absorbing < ~350nm