PECVD Recipes: Difference between revisions
Jump to navigation
Jump to search
Content deleted Content added
| Line 99: | Line 99: | ||
*[https://docs.google.com/spreadsheets/d/1GZ58eFzD-T8DJ2Nsaj74u6cvawzsOI2DmMit6Z7vqys/edit#gid=sharing LS Nitride2 Data 2016] |
*[https://docs.google.com/spreadsheets/d/1GZ58eFzD-T8DJ2Nsaj74u6cvawzsOI2DmMit6Z7vqys/edit#gid=sharing LS Nitride2 Data 2016] |
||
*[https://docs.google.com/spreadsheets/d/1gGIWqkCnykPgBc3prhXExT7QcNjWm2HdbTtwugNqm18/edit#gid=sharing LS Nitride2 Data 2017] |
*[https://docs.google.com/spreadsheets/d/1gGIWqkCnykPgBc3prhXExT7QcNjWm2HdbTtwugNqm18/edit#gid=sharing LS Nitride2 Data 2017] |
||
*[https://docs.google.com/spreadsheets/d/1vwpDtiglR2DLWiYNhpBX77cyyj9lw55iVeFz1puN7bM/edit#gid=sharing LS |
*[https://docs.google.com/spreadsheets/d/1vwpDtiglR2DLWiYNhpBX77cyyj9lw55iVeFz1puN7bM/edit#gid=sharing LS Nitride2 Data 2018] |
||
*[https://docs.google.com/spreadsheets/d/1zvSl2P5T926Ol48yH3FBCZm1zCeycl3S8GWQYtzi8VI/edit#gid=sharing LS |
*[https://docs.google.com/spreadsheets/d/1zvSl2P5T926Ol48yH3FBCZm1zCeycl3S8GWQYtzi8VI/edit#gid=sharing LS Nitride2 Data 2019] |
||
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness Uniformity 2014] |
*[https://docs.google.com/spreadsheet/ccc?key=0AnwBU1s4JQo2dENSak1ZNnVaVTFEQTBzdDJMSDlDTFE&usp=drive_web#gid=1=sharing LS Nitride2 Thickness Uniformity 2014] |
||
Revision as of 21:20, 2 January 2019
Back to Vacuum Deposition Recipes.
PECVD 1 (PlasmaTherm 790)
Note: Software upgrade performed on 2018-10-10. Note any changes in film.
- Particulates (Gain4) in PECVD#1 2015
- Particulates (Gain4) in PECVD#1 2016
- Particulates (Gain4) in PECVD#1 2017
SiN deposition (PECVD #1)
- SiN Standard Recipe
- SiN 100nm Data 2014
- SiN 100nm Data 2015
- SiN 100nm Data 2016
- SiN 100nm Data 2017
- SiN 300nm Data 2017
- SiN 300nm Data 2018
- SiN 100 nm Thickness uniformity 2014
- SiN 100 nm Thickness uniformity 2015
- SiN 100 nm Thickness uniformity 2016
- SiN 100 nm Thickness uniformity 2017
- SiN 300nm Thickness uniformity 2017
- SiN 300nm Thickness uniformity 2018
SiO2 deposition (PECVD #1)
- SiO2 Standard Recipe
- SiO2 100nm Data 2014
- SiO2 100nm Data 2015
- SiO2 100nm Data 2016
- SiO2 100nm Data 2017
- SiO2 300nm Data 2017
- SiO2 300nm Data 2018
- SiO2 100nm Thickness uniformity 2014
- SiO2 100 nm Thickness uniformity 2015
- SiO2 100 nmThickness uniformity 2016
- SiO2 100nm Thickness uniformity 2017
- SiO2 300nm Thickness uniformity 2017
- SiO2 300nm Thickness uniformity 2018
OTHER recipes: Low-Stress (LS) SiN and SiOxNy deposition (PECVD #1)
- LS SiN Standard Recipe
- LS SiN Data 2014
- LS SiN 1000A Thickness uniformity 2014
- SiOxNy Standard Recipe
- SiOxNy Data 2014
- SiOxNy1000A Thickness uniformity 2014
PECVD 2 (Advanced Vacuum)
- Particulates (Gain4) in PECVD#2 2015
- Particulates (Gain4) in PECVD#2 2016
- Particulates (Gain4) in PECVD#2 2017
SiO2 deposition (PECVD #2)
- Oxide Standard Recipe
- Oxide Data 2014
- Oxide Data 2015
- Oxide data 2016
- Oxide Data 2017
- Oxide Data 2018
- Oxide Thickness Uniformity 2014
- Oxide Thickness Uniformity 2015
- Oxide Thickness Uniformity 2016
- Oxide Thickness Uniformity 2017
- Oxide Thickness Uniformity 2018
SiN deposition (PECVD #2)
- Nitride2 Standard Recipe
- Nitride2 Data 2014
- Nitride2 Data 2015
- Nitride2 Data 2016
- Nitride2 Data 2017
- Nitride2 Data 2018
- Nitride2 Thickness Uniformity 2014
- Nitride2 Thickness Uniformity 2015
- Nitride2 Thickness Uniformity 2016
- Nitride2 Thickness Uniformity 2017
- Nitride2 Thickness Uniformity 2018
- SiNx Film Stress vs LF and HF Duration Time, and Gas Flowing-rate
Low-Stress SiN deposition (PECVD #2)
Low-Stress SilIcon Nitride (< 100 MPa)
- LS Nitride2 Data 2014
- LS Nitride2 Data 2015
- LS Nitride2 Data 2016
- LS Nitride2 Data 2017
- LS Nitride2 Data 2018
- LS Nitride2 Data 2019
- LS Nitride2 Thickness Uniformity 2014
- LS Nitride2 Thickness Uniformity 2015
- LS Nitride2 Thickness Uniformity 2016
- LS Nitride2 Thickness Uniformity 2017
- LS Nitride2 Thickness Uniformity 2018
Amorphous-Si deposition (PECVD #2)
ICP-PECVD (Unaxis VLR)
SiN deposition (Unaxis VLR)
SiN (2% SiH4)
SiN (2% SiH4 - No-Ar)
SiN (2% SiH4 - No-Ar - Extra N2)
| 50° (pinholes) | 100° (pinholes) | 250° |
|---|---|---|
SiN (100% SiH4 )
| 50° (pinholes) | 100° (pinholes) | 250° |
|---|---|---|
SiO2 deposition (Unaxis VLR)
SiO2 (2% SiH4)
| 50° | 100° | 250° |
|---|---|---|
SiO2 (2% SiH4 - No Ar)
| 50° | 100° | 250° |
|---|---|---|
SiO2 (100% SiH4 HDR)
| 50° | 100° | 250° |
|---|---|---|
SiO2 (100% SiH4 LDR)
| 50° | 100° | 250° |
|---|---|---|
Amorphous Si (100%SiH4 Ar He)
| 90° | 250° |
|---|---|