Stepper 3 (ASML DUV): Difference between revisions
m (→Online Video Trainings: disclaimer about supervisor training) |
(→Online Video Trainings: privatized the Video Trianings, note on how to reaquire access.) |
||
(32 intermediate revisions by 2 users not shown) | |||
Line 4: | Line 4: | ||
|super= Demis D. John |
|super= Demis D. John |
||
|location=Bay 7 |
|location=Bay 7 |
||
|description = |
|description = Deep-UV Stepper Photolithography |
||
|model = PAS 5500/300 |
|||
|manufacturer = [http://www.asml.com ASML] |
|manufacturer = [http://www.asml.com ASML] |
||
|ToolType = Lithography |
|ToolType = Lithography |
||
Line 14: | Line 15: | ||
==About== |
==About== |
||
===General Capabilities/Overview=== |
|||
The ASML 5500 stepper is a 248nm DUV stepper for imaging dense features down to below 200nm and isolated line structures down to below 150nm. Overlay accuracy is better than 30nm. |
|||
The ASML 5500 stepper is a 248nm (KrF) DUV stepper for imaging dense features down to below 200nm and isolated line structures down to below 150nm (with effort). 300nm features are relatively "easy" to resolve. Layer-to-layer overlay accuracy is better than 30nm. |
|||
The system is configured for 4” wafers |
The system is configured for 4” wafers. The system is designed for high throughput, so shooting multiple 4" wafers is extremely fast, typically minutes per wafer, but any size other than 4-inch is difficult to work with (see below for more info). Additionally, exposure jobs are highly programmable, allowing for very flexible exposures of multiple aligned patterns from multiple masks/reticles in a single session, allowing for process optimization of large vs. small features in a single lithography. |
||
The full field useable exposure area is limited to the intersection of a 31mm diameter circle and a rectangle of dimensions 22mm x 27mm. See the [[ASML 5500 Mask Making Guidelines|Mask Making Guidelines page]] for more info on exposure field sizes and how to order your mask plates. |
The full field useable exposure area is limited to the intersection of a 31mm diameter circle and a rectangle of dimensions 22mm x 27mm. Users have stitched multiple photomasks together with success. See the [[ASML 5500 Mask Making Guidelines|Mask Making Guidelines page]] for more info on exposure field sizes and how to order your mask plates. |
||
===Photoresists Available=== |
|||
Resists Used (see [https://wiki.nanotech.ucsb.edu/wiki/index.php/Lithography_Recipes#Photolithography_Recipes PhotoLith. Recipes] for full process info): |
|||
''See [https://wiki.nanotech.ucsb.edu/w/index.php?title=Lithography_Recipes#Photolithography_Recipes PhotoLith. Recipes] for full process info & links to PR datasheets.'' |
|||
*UV210-0.3 - Positive: 300nm nominal thickness |
*UV210-0.3 - Positive: 300nm nominal thickness |
||
Line 31: | Line 34: | ||
AZ300MIF Developer for all processes |
AZ300MIF Developer for all processes |
||
Many of these DUV PR's are also able to be exposed with [[E-Beam Lithography System (JEOL JBX-6300FS)|EBL]]. |
|||
===Part Size Limits=== |
|||
With staff support, mounted pieces down to 14mm in size can be exposed using a 4” wafer as a carrier. Flatness will typically be worse in this situation, so small <<500nm features will usually have bad uniformity across the mounted part due to focus variations. Edge bead on irregular pieces (eg. quarter-wafers/squares) will significantly reduce yield/uniformity. |
|||
Multi-layer Alignment on mounted parts is particularly difficult, requiring either semi-permanent mounting to the carrier (eg. BCB, SU8 etc.) or significant difficulty/effort to re-align the part to the carrier wafer on each lithography (≤100µm re-mounting accuracy needed). |
|||
At this time the maximum wafer size is 4” (100mm) wafers with SEMI standard wafer flat (not Notch). |
|||
===Service Provider=== |
|||
*[http://www.asml.com ASML] - ASML performs quarterly periodic maintenance and provides on-demand support. |
|||
==Process Information== |
==Process Information== |
||
*[https://wiki.nanotech.ucsb.edu/ |
*[https://wiki.nanotech.ucsb.edu/w/index.php?title=Lithography_Recipes#Photolithography_Recipes '''Process Recipes Page'''] '''> "Stepper 3"''' - ''Established recipes and corresponding linewidths, photoresists etc.'' |
||
*Sample size: 100 mm wafers with SEMI std. major flat |
*Sample size: 100 mm wafers with SEMI std. major flat |
||
**''Piece-parts process is possible but difficult - contact |
**''Piece-parts process is possible but difficult - contact supervisor for info'' |
||
*Alignment Accuracy: < 50 nm |
*Alignment Accuracy: < 50 nm |
||
*Minimum Feature Size: ≤150 nm isolated lines, ≤200 nm dense patterns |
*Minimum Feature Size: ≤150 nm isolated lines, ≤200 nm dense patterns |
||
**''To achieve ≤200nm features with high uniformity, we recommend wafers with total thickness variation (TTV) ≤5µm, and designing your CAD with a smaller Image Size for the high-res. feature''. |
|||
*Maximum Wafer Bow: approx. 100 µm. (4-inch diam.) |
|||
*Wafer Thickness: Minimum ≈ 200µm, Maximum ≈ 1.1 mm |
|||
**''Near this value, and the job may fail or lose the wafer inside the machine due to wafer vacuum error.'' |
|||
*Maximum Dose: ~100mJ |
|||
**''Non-chemically amplified EBL resists are not permissible due to this limit.'' |
|||
*Maximum Wafer Bow (measured over 90mm on the [[Film Stress (Tencor Flexus)|Tencor Flexus]]): |
|||
**'''Do not run wafers with bow values higher than the following values''', contact supervisor for advice if needed. |
|||
**Silicon wafers (~550µm thick): 100 µm will likely fail. |
|||
**Sapphire (less pliable), ≥60µm bow will intermittently fail. |
|||
***This applies especially for GaN-on-Sapphire, whcih often have high wafer bow. |
|||
**''Near these values, and you may lose the wafer inside the machine due to wafer vacuum error.'' |
|||
**''Substrate material and substrate thickness affect this limit - please contact supervisor for advice.'' |
|||
**You can stress-compensate wafers to reduce the wafer bow, eg. via underside dep. of [[Sputtering Recipes#Si3N4 deposition .28IBD.29|IBD SiN]], or other compressive/tensile films for concave-down/up bow, respectively. |
|||
==Operating Procedures== |
==Operating Procedures== |
||
Line 46: | Line 72: | ||
*[[ASML Stepper 3 Standard Operating Procedure|Standard Operating Procedures]] - ''Exposing wafers, loading reticles, focus/exposure matrix'' |
*[[ASML Stepper 3 Standard Operating Procedure|Standard Operating Procedures]] - ''Exposing wafers, loading reticles, focus/exposure matrix'' |
||
**[[ASML Stepper 3 Standard Operating Procedure#Running a focus and.2For exposure matrix|Focus-Exposure Matrix]] - ''used for'' ''calibrating sensitive exposure parameters'' |
**[[ASML Stepper 3 Standard Operating Procedure#Running a focus and.2For exposure matrix|Focus-Exposure Matrix]] - ''used for'' ''calibrating sensitive exposure parameters'' |
||
*[[ASML Stepper 3 Error Recovery, Troubleshooting and Calibration|Error Recovery, Troubleshooting & Calibration Check]] |
|||
**''Common errors/solutions, System Calibration Verification (aka. IQC)'' |
|||
*[[ASML 5500: Recovering from an Error|ASML 5500: Recovering from an Error+Wafer Retrieval]] |
|||
**''How to abort the job and recover your wafer.'' |
|||
*[//wiki.nanotech.ucsb.edu/wiki/images/c/cd/ASML_Job_Set-Up_Guide_simple_v1.pdf Job Programming- Simplified - Full Wafers] |
|||
*[//wiki.nanotech.ucsb.edu/wiki/images/f/f7/ASML_Job_Set-Up_Guide_v2.pdf Job Programming - Full] |
*[//wiki.nanotech.ucsb.edu/wiki/images/f/f7/ASML_Job_Set-Up_Guide_v2.pdf Job Programming - Full] |
||
*[//wiki.nanotech.ucsb.edu/wiki/images/c/cd/ASML_Job_Set-Up_Guide_simple_v1.pdf Job Programming- Simplified -Full Wafers] |
|||
*[[ASML Stepper 3 - Substrates smaller than 100mm/4-inch|Working with Substrates Smaller than 100mm/4-inch]] |
|||
=== Online Video Trainings === |
|||
*[[ASML 5500 Mask Making Guidelines|Mask Making Guidelines]] |
|||
**''All the info you need to design and order a reticle for this system.'' |
|||
===Training Procedure=== |
|||
To get access to this tool, please do the following: |
|||
#Email the [[Demis D. John|supervisor]] for access to the training video. Please provide your UCSB NetID. |
|||
#Study the training videos below. |
|||
##If you are a technician and will never program jobs, only Part 1 is necessary. |
|||
#"Shadow" someone in your group who uses the machine, <u>until you are completely comfortable</u> with wafer cleaning (critical), reticle load/unload and running a pre-made job. When you are ready do step 3: |
|||
#Contact [[Demis D. John|the supervisor]] for an short hands-on check-off, after which you'll get signupmonkey access. |
|||
===Online Video Trainings=== |
|||
The video trainings are only accessible to authorized users per vendor request. Email the [[Demis D. John|supervisor]] for access. |
|||
''These video trainings have bookmarks to skip to specific sections - use them as reference.'' |
''These video trainings have bookmarks to skip to specific sections - use them as reference.'' |
||
''Remember, you are NOT authorized to use the system until a supervisor grants you access.'' |
''Remember, you are NOT authorized to use the system until a [[Demis D. John|supervisor]] grants you access.'' |
||
* [[To Be Added|Part 1: Running a Job]] |
|||
* [https://gauchocast.hosted.panopto.com/Panopto/Pages/Viewer.aspx?id=dc501ba5-1f20-401c-8a96-ac2500f7e81e Part 2: Job Programming] |
|||
View on "'''''GauchoSpace"''''' ''(not "Panopto"), with your authorized UCSB NetID'': |
|||
===Troubleshooting and Recovery=== |
|||
*[https://gauchocast.hosted.panopto.com/Panopto/Pages/Viewer.aspx?id=798e5110-0823-4abd-9458-ac5c01855a99 Part 1: System Info & Running a Job] |
|||
*[[ASML Stepper 3 Error Recovery, Troubleshooting and Calibration|Error Recovery, Troubleshooting and Calibration]] |
|||
*[https://gauchocast.hosted.panopto.com/Panopto/Pages/Viewer.aspx?id=dc501ba5-1f20-401c-8a96-ac2500f7e81e Part 2: Job Programming] |
|||
**''Common errors/System Warnings, Wafer Handler Reset, System Calibration Verification'' |
|||
==Design Tools== |
|||
*[[ASML 5500: Recovering from an Error|ASML 5500: Recovering from an Error/Wafer Retrieval]] |
|||
**''How to abort the job and recover your wafer.'' |
|||
*[https://github.com/demisjohn/ASML_JobCreator ASML Job Creator] - Python scripts for generating ASML Job Files. |
|||
**''Remotely-uploadable job scripting is now possible - contact [[Demis D. John|the supervisor]] if interested.'' |
|||
**'''''<code>Note: Automated Upload/conversion is disabled due to system software upgrades - we are working to restore this. 2022-09 [[Demis D. John|DJ]]</code>''''' |
|||
*[[ASML Stepper 3 - UCSB Test Reticles|UCSB DUV Reticles]] - Photomasks available with various Alignment Markers (contact, EBL), Resolution Testing etc. |
|||
===Mask Design and CAD files=== |
|||
*[[ASML 5500 Mask Making Guidelines|Mask Making Guidelines]] - All the info you need to design and order a reticle for this system. |
|||
*[[ASML 5500 Mask Making Guidelines#Templates|Templates and CAD help]] - on the above page, CAD files and spreadsheets to help you design/program. |
|||
*See the [[Calculators + Utilities#CAD%20Files%20.26%20Templates|Calculators + Utilities > CAD Files & Templates]] page for other useful CAD files, such as overlay verniers, vented fonts etc. |
|||
===Software Options=== |
===Software Options=== |
||
''The Following software options have been installed on the machine.'' |
|||
*[[ASML Stepper 3 - Shifted Measurement Scans (SMS)|Shifted Measurement Scans]] - better tilt/level measurement locations for edge-die. Simply enable the Checkbox in your job file. |
*[[ASML Stepper 3 - Shifted Measurement Scans (SMS)|Shifted Measurement Scans]] - better tilt/level measurement locations for edge-die. Simply enable the Checkbox in your job file. |
||
*[[ASML Stepper 3 - Compound Image Design (CIDS)|Compound Image Design]] - flexible Image Distribution: grouping of Images with shifts, duplicate instances of Images in each Cell. |
*[[ASML Stepper 3 - Compound Image Design (CIDS)|Compound Image Design]] - flexible Image Distribution: grouping of Images with shifts, duplicate instances of Images in each Cell. |
||
*[[ASML Stepper 3 - Job Creator|Job Creator]] - create binary ASML job files from ASCII text files. Python scripting capabilities using this option are currently implemented, |
*[[ASML Stepper 3 - Job Creator|Job Creator]] - create binary ASML job files from ASCII text files. Python scripting capabilities using this option are currently implemented, contact [[Demis D. John|the supervisor]] for more info. |
||
==Recipes== |
|||
==Design & Fabrication Tools== |
|||
*[[ASML 5500 Mask Making Guidelines|ASML 5500 Mask Making Guidelines]] - All the info you need to design and order a reticle for this system. |
|||
**[[ASML 5500 Mask Making Guidelines#Templates|Templates and CAD help]] - on the above page, CAD files and spreadsheets to help you design/program. |
|||
*[https://github.com/demisjohn/ASML_JobCreator ASML Job Creator] - Python scripts for generating ASML Job Files. |
|||
**''This new scriptable job programming is in the user-testing phase - contact [[Demis D. John|the supervisor]] if interested.'' |
|||
*[[ASML Stepper 3 - UCSB Test Reticles|UCSB Test Reticles]] - Alignment Markers, Resolution Testing etc. |
|||
== Recipes == |
|||
See the '''[[Stepper Recipes#Stepper 3 .28ASML DUV.29|Recipes > Lithography > Stepper Recipes > Stepper #3]]''' page for starting processes for various photoresists, including Dose/Focus values. |
See the '''[[Stepper Recipes#Stepper 3 .28ASML DUV.29|Recipes > Lithography > Stepper Recipes > Stepper #3]]''' page for starting processes for various photoresists, including Dose/Focus values. |
||
Litho. recipes for all our photolith. tools can be found on the [[Lithography Recipes#Photolithography Recipes|Photolithography Recipes]] page. |
Litho. recipes for all our photolith. tools can be found on the [[Lithography Recipes#Photolithography Recipes|Photolithography Recipes]] page. |
||
== |
==Process Control Data== |
||
*''The Process Group regularly measures data on lithography Critical Dimension ("CD") and Wafer-stage Particulate Contamination for this tool, using a sensitive lithography process that will reveal small changes in Dose repeatability and wafer flatness.'' |
|||
*[http://www.asml.com ASML] - ASML performs quarterly periodic maintenance and provides on-demand support. |
|||
*[https://docs.google.com/spreadsheets/d/1xW1TFH_QjPMWl9T1jiKzwmYe4B2wg7KY-nqOKUoXttI/edit#gid=0 '''Data Table for CD Uniformity and Particulate Contamination'''] |
|||
*[https://docs.google.com/spreadsheets/d/1xW1TFH_QjPMWl9T1jiKzwmYe4B2wg7KY-nqOKUoXttI/edit#gid=1804752281 '''Plots of CD Repeatability'''] |
|||
{| |
|||
|[[File:ASML CD Cals - Example Table.jpg|alt=ASML CD Calibration data - Screenshot of Table|none|thumb|300x300px|''Example of Data Table with SEM's of 320nm features. [https://docs.google.com/spreadsheets/d/1xW1TFH_QjPMWl9T1jiKzwmYe4B2wg7KY-nqOKUoXttI/edit#gid=0 Click for full data table.]''|link=https://docs.google.com/spreadsheets/d/1xW1TFH_QjPMWl9T1jiKzwmYe4B2wg7KY-nqOKUoXttI/edit#gid=0]] |
|||
|[[File:ASML CD Cals - Example Plot.jpg|alt=ASML CD Calibration Data - Screenshot of SPC Plot|none|thumb|''Example SPC Chart - Measured Critical Dimension "CD" versus Date. [https://docs.google.com/spreadsheets/d/1xW1TFH_QjPMWl9T1jiKzwmYe4B2wg7KY-nqOKUoXttI/edit#gid=1804752281 Click for charts.]''|link=https://docs.google.com/spreadsheets/d/1xW1TFH_QjPMWl9T1jiKzwmYe4B2wg7KY-nqOKUoXttI/edit#gid=1804752281]] |
|||
|} |
|||
<br /> |
Revision as of 21:51, 29 September 2023
|
About
General Capabilities/Overview
The ASML 5500 stepper is a 248nm (KrF) DUV stepper for imaging dense features down to below 200nm and isolated line structures down to below 150nm (with effort). 300nm features are relatively "easy" to resolve. Layer-to-layer overlay accuracy is better than 30nm.
The system is configured for 4” wafers. The system is designed for high throughput, so shooting multiple 4" wafers is extremely fast, typically minutes per wafer, but any size other than 4-inch is difficult to work with (see below for more info). Additionally, exposure jobs are highly programmable, allowing for very flexible exposures of multiple aligned patterns from multiple masks/reticles in a single session, allowing for process optimization of large vs. small features in a single lithography.
The full field useable exposure area is limited to the intersection of a 31mm diameter circle and a rectangle of dimensions 22mm x 27mm. Users have stitched multiple photomasks together with success. See the Mask Making Guidelines page for more info on exposure field sizes and how to order your mask plates.
Photoresists Available
See PhotoLith. Recipes for full process info & links to PR datasheets.
- UV210-0.3 - Positive: 300nm nominal thickness
- UV6-0.8 - Positive: 800nm nominal thickness
- UV26-2.5 - Positive: 2.5um nominal thickness
- UVN2300-0.5 - Negative: 500nm nominal thickness
- DUV42P-6/DS-K101 - Bottom Anti-Reflective Coatings “BARC”
- PMGI/LOL1000/LOL2000 - Underlayers
AZ300MIF Developer for all processes
Many of these DUV PR's are also able to be exposed with EBL.
Part Size Limits
With staff support, mounted pieces down to 14mm in size can be exposed using a 4” wafer as a carrier. Flatness will typically be worse in this situation, so small <<500nm features will usually have bad uniformity across the mounted part due to focus variations. Edge bead on irregular pieces (eg. quarter-wafers/squares) will significantly reduce yield/uniformity.
Multi-layer Alignment on mounted parts is particularly difficult, requiring either semi-permanent mounting to the carrier (eg. BCB, SU8 etc.) or significant difficulty/effort to re-align the part to the carrier wafer on each lithography (≤100µm re-mounting accuracy needed).
At this time the maximum wafer size is 4” (100mm) wafers with SEMI standard wafer flat (not Notch).
Service Provider
- ASML - ASML performs quarterly periodic maintenance and provides on-demand support.
Process Information
- Process Recipes Page > "Stepper 3" - Established recipes and corresponding linewidths, photoresists etc.
- Sample size: 100 mm wafers with SEMI std. major flat
- Piece-parts process is possible but difficult - contact supervisor for info
- Alignment Accuracy: < 50 nm
- Minimum Feature Size: ≤150 nm isolated lines, ≤200 nm dense patterns
- To achieve ≤200nm features with high uniformity, we recommend wafers with total thickness variation (TTV) ≤5µm, and designing your CAD with a smaller Image Size for the high-res. feature.
- Wafer Thickness: Minimum ≈ 200µm, Maximum ≈ 1.1 mm
- Maximum Dose: ~100mJ
- Non-chemically amplified EBL resists are not permissible due to this limit.
- Maximum Wafer Bow (measured over 90mm on the Tencor Flexus):
- Do not run wafers with bow values higher than the following values, contact supervisor for advice if needed.
- Silicon wafers (~550µm thick): 100 µm will likely fail.
- Sapphire (less pliable), ≥60µm bow will intermittently fail.
- This applies especially for GaN-on-Sapphire, whcih often have high wafer bow.
- Near these values, and you may lose the wafer inside the machine due to wafer vacuum error.
- Substrate material and substrate thickness affect this limit - please contact supervisor for advice.
- You can stress-compensate wafers to reduce the wafer bow, eg. via underside dep. of IBD SiN, or other compressive/tensile films for concave-down/up bow, respectively.
Operating Procedures
- Standard Operating Procedures - Exposing wafers, loading reticles, focus/exposure matrix
- Focus-Exposure Matrix - used for calibrating sensitive exposure parameters
- Error Recovery, Troubleshooting & Calibration Check
- Common errors/solutions, System Calibration Verification (aka. IQC)
- ASML 5500: Recovering from an Error+Wafer Retrieval
- How to abort the job and recover your wafer.
- Job Programming- Simplified - Full Wafers
- Job Programming - Full
- Mask Making Guidelines
- All the info you need to design and order a reticle for this system.
Training Procedure
To get access to this tool, please do the following:
- Email the supervisor for access to the training video. Please provide your UCSB NetID.
- Study the training videos below.
- If you are a technician and will never program jobs, only Part 1 is necessary.
- "Shadow" someone in your group who uses the machine, until you are completely comfortable with wafer cleaning (critical), reticle load/unload and running a pre-made job. When you are ready do step 3:
- Contact the supervisor for an short hands-on check-off, after which you'll get signupmonkey access.
Online Video Trainings
The video trainings are only accessible to authorized users per vendor request. Email the supervisor for access.
These video trainings have bookmarks to skip to specific sections - use them as reference.
Remember, you are NOT authorized to use the system until a supervisor grants you access.
View on "GauchoSpace" (not "Panopto"), with your authorized UCSB NetID:
Design Tools
- ASML Job Creator - Python scripts for generating ASML Job Files.
- Remotely-uploadable job scripting is now possible - contact the supervisor if interested.
Note: Automated Upload/conversion is disabled due to system software upgrades - we are working to restore this. 2022-09 DJ
- UCSB DUV Reticles - Photomasks available with various Alignment Markers (contact, EBL), Resolution Testing etc.
Mask Design and CAD files
- Mask Making Guidelines - All the info you need to design and order a reticle for this system.
- Templates and CAD help - on the above page, CAD files and spreadsheets to help you design/program.
- See the Calculators + Utilities > CAD Files & Templates page for other useful CAD files, such as overlay verniers, vented fonts etc.
Software Options
The Following software options have been installed on the machine.
- Shifted Measurement Scans - better tilt/level measurement locations for edge-die. Simply enable the Checkbox in your job file.
- Compound Image Design - flexible Image Distribution: grouping of Images with shifts, duplicate instances of Images in each Cell.
- Job Creator - create binary ASML job files from ASCII text files. Python scripting capabilities using this option are currently implemented, contact the supervisor for more info.
Recipes
See the Recipes > Lithography > Stepper Recipes > Stepper #3 page for starting processes for various photoresists, including Dose/Focus values.
Litho. recipes for all our photolith. tools can be found on the Photolithography Recipes page.
Process Control Data
- The Process Group regularly measures data on lithography Critical Dimension ("CD") and Wafer-stage Particulate Contamination for this tool, using a sensitive lithography process that will reveal small changes in Dose repeatability and wafer flatness.
- Data Table for CD Uniformity and Particulate Contamination
- Plots of CD Repeatability
![]() Example of Data Table with SEM's of 320nm features. Click for full data table. |
![]() Example SPC Chart - Measured Critical Dimension "CD" versus Date. Click for charts. |