Stepper 2 (AutoStep 200): Difference between revisions

From UCSB Nanofab Wiki
Jump to navigation Jump to search
Content deleted Content added
Biljana (talk | contribs)
→Operating Procedures: link to Job Programming
No edit summary
 
(110 intermediate revisions by 5 users not shown)
Line 1: Line 1:
{{tool|{{PAGENAME}}
{{tool2_DJ|{{PAGENAME}}
|picture=Stepper2.jpg
|picture=Stepper2.jpg
|type = Lithography
|type = Lithography
|super= Biljana Stamenic
|super= Biljana Stamenic
|super2 = Bill Millerski
|phone=(805)839-3918x213
|location=Bay 6
|location=Bay 6
|email=biljana@ece.ucsb.edu
|description = GCA 200 I-Line Wafer Stepper
|description = GCA 200 I-Line Wafer Stepper
|manufacturer = GCA
|manufacturer = GCA
|materials =
|materials =
|recipe = Lithography
|toolid=38
|toolid=38
}}
}}
{{ToolActions
|toolid = 38
|ProcessControlURL =
|ProceduresURL =
|TrainingURL = Stepper_2_(AutoStep_200)#Video_Training
}}


== About ==
==About==


Our GCA wafer stepper is an i-line (365 nm) step and repeat exposure tool for doing lithography that requires high resolution (≥500nm) and/or critical alignment (≥150nm).
Our GCA wafer stepper is an i-line (365 nm) step and repeat exposure tool for doing lithography that requires high resolution and/or critical alignment. The system has been modified to accept piece parts (down to smaller than 10mm x 10mm) up to 6” diameter wafers using manual wafer loading. The maximum square die size is 14.8 mm x 14.8 mm. The system has an Olympus 2145 (N.A. = 0.45) lens that reduces the mask image by 5 x and gives an ultimate resolution of better than 0.5 um in the center of the lens field. The system can easily produce 0.7 um isolated lines across the entire field. The Autostep200 system has 3-point wafer leveling to improve focus uniformity across the field. Autofocus is used to determine the sample surface relative to the lens, making the focus stable and repeatable for different thickness of wafer. The stages are controlled by stepper motors and laser interferometers. Using the global, manual alignment, better than 0.25 um alignment error is achievable. Using the DFAS local alignment system, alignment error better than 0.15 um is achieved. With the 1000 W Hg arc lamp, we get about 420 mW/cm² of i-line intensity at the wafer.

The system has been modified to accept piece parts (down to smaller than 10mm x 10mm) up to 6” diameter wafers using manual wafer loading. The maximum square die size is 14.8 mm x 14.8 mm.

The system has an Olympus 2145 (N.A. = 0.45) lens that reduces the mask image by 5x and gives an ultimate resolution of better than 0.5 um in the center of the lens field. The system can easily produce 0.7 um isolated lines across the entire field. The Autostep200 system has 3-point wafer leveling to improve focus uniformity across the field. Autofocus is used to determine the sample surface relative to the lens, making the focus stable and repeatable for different thickness of wafer. The stages are controlled by stepper motors and laser interferometers.

Using the "global", manual alignment, better than 0.25 um alignment error is achievable. Using the DFAS "local" alignment system, alignment error better than 0.15 um is achieved. With the 1000 W Hg arc lamp, we get about 420 mW/cm² of i-line intensity at the wafer.


The system is computer controlled with the capability to program and save a wide variety of exposure jobs. We also have unlimited phone support for system problems through a service contract.
The system is computer controlled with the capability to program and save a wide variety of exposure jobs. We also have unlimited phone support for system problems through a service contract.


'''Tutorial:''' If you are not familiar with the differences between Contact Litho and Stepper Litho, please review this short tutorial: [https://wiki.nanofab.ucsb.edu/w/images/c/cb/Demis_D_John_-_Stepper_Reticle_Layout_vs_Wafer_Layout.pdf Demis D. John - Stepper_Reticle_Layout_vs_Wafer_Layout.pdf]

* Explains how a Stepper mask can have ''many'' designs, and flexibly pattern the wafer with combos of designs.


==Detailed Specifications==
==Detailed Specifications==

*Lens: Olympus 2145: NA = 0.45; Depth of field = 1.2 um for 0.6 um process
*Lens: Olympus 2145: NA = 0.45; Depth of field = 1.2 um for 0.6 um process
*Maximum die size: ~ 15 mm x 15 mm
*Maximum die size: ~ 15 mm x 15 mm
*Maximum substrate thickness: we have various chucks with shims to allow different thicknesses - contact staff for info.
*Up to 4 lithography images per reticle, with maximum size of ~7.5 x 7.5 mm each.
*Resolution: 400-450 nm for R&D; 700 nm over entire 15 mm x 15 mm field
*Resolution: 400-450 nm for R&D; 700 nm over entire 15 mm x 15 mm field
*Registration tolerance: 0.25 µm global alignment; Max 0.15 µm local alignment (with care, you can achieve < 0.10 µm registration)
*Registration tolerance: 0.25 µm global alignment; Max 0.15 µm local alignment (with care, you can achieve < 0.10 µm registration)
Line 27: Line 45:
*Computer programmable, recipes saved on hard disk
*Computer programmable, recipes saved on hard disk
*Reticle alignment fiducials and global/local fiducials available - contact us for CAD files.
*Reticle alignment fiducials and global/local fiducials available - contact us for CAD files.
*Mask Plates: 5x5x0.090 inches, 5x reduction, typically Soda Lime Glass (Quartz is also acceptable), no pellicle.


== Process Information ==
==Process Information==


===Photomask Info===
*[https://signupmonkey.ece.ucsb.edu/wiki/index.php/Lithography_Recipes#Photolithography_Recipes Process Page: Photolithography Recipes]


*[[Autostep 200 Mask Making Guidance]] - ''information on designing and ordering your photomasks for this system.''
=== Photoresists: ===

*The laboratory contains a variety of i-line compatible photoresists. See the [https://signupmonkey.ece.ucsb.edu/wiki/index.php/Lithography_Recipes#Photolithography_Recipes Photolith. Recipes Page] for detailed processing info (bakes/spins/exposure does etc.). Basic photoresists include:
===Recipes===
**955CM-0.9 for 0.7-1.0 um thick positive processes.

**AZ5214E for 1.0 um thick image reversal (negative) process.

**SPR955CM-1.8 for 1.5-2.0 um thick positive processes.
*[https://wiki.nanofab.ucsb.edu/wiki/Stepper_Recipes#Stepper_2_.28AutoStep_200.29 Photolitography Recipes]*
**SPR220-3 for 2.5-5 um thick positive process.

**SPR220-7 for >5 um thick positive processes.
===Photoresists===
**AZnLOF5510 for <1.0um and AZnLOF 2020 for 1.5-3 um negative resist process.

*The laboratory contains a variety of i-line compatible photoresists. See the [https://signupmonkey.ece.ucsb.edu/w/index.php?title=Lithography_Recipes#Photolithography_Recipes Photolith. Recipes Page] for detailed processing info (bakes/spins/exposure does etc.). Basic photoresists include:
**955CM-0.9 for 0.7-1.0 um thick positive processes.
**AZ5214E for 1.0 um thick image reversal (negative) process.
**SPR955CM-1.8 for 1.5-2.0 um thick positive processes.
**SPR220-3 for 2.5-5 um thick positive process.
**SPR220-7 for >5 um thick positive processes.
**AZnLOF5510 for <1.0um and AZnLOF 2020 for 1.5-3 um negative resist process.
**Shipley LOL-2000 is also used as an underlayer for high resolution lift-off processes.
**Shipley LOL-2000 is also used as an underlayer for high resolution lift-off processes.

===CAD Files===

*[[Media:GCA Stepper MaskPlate Master-DarkField 5x.gds|Photomask Template: Dark-field (polygons/objects are clear) at 5x Magnification (GDS)]]
**''This template is designed to be submitted to the photomask vendor to print as-is, no scaling applied.''
**''Insert your designs into the template as Instances scaled UP by 5x.''
*[[Media:GCA Global Mark.gds|Global Alignment Mark CAD File (GDS)]]
*[[Media:GCA Local Alignment Mark.gds|Local Alignment Mark CAD File (GDS)]]
*[[Media:GCA Local Alignment Mark Dotted.gds|Local Alignment Mark CAD File: Dotted (GDS)]]
**''This dotted version works for low-contrast layers (eg. mark etched into very thin ≤100nm layer).''
*See the [[Calculators + Utilities#CAD%20Files%20.26%20Templates|Calculators + Utilities > CAD Files & Templates]] page for other useful CAD files, such as overlay verniers, vented fonts etc.


==Service Provider==
==Service Provider==

* [http://3ctechnical.com/index.html 3C Technical] - The company that services the stepper.
*[http://3ctechnical.com/index.html 3C Technical] - The company that services the stepper.


==Operating Procedures==
==Operating Procedures==

* [[media:Autostep 200 Training Manual-4-10-15 .pdf|Training Manual]]
===Tool Operation===
* [[Stepper 2 (Autostep 200) - Job Programming|Programming a Job]]

*[https://wiki.nanofab.ucsb.edu/w/images/0/05/Running_the_JOB-_One_Page_Instructions.pdf Running the JOB - One Page Instructions]
*[https://wiki.nanofab.ucsb.edu/w/images/f/f3/Autostep_200_-_Standard_Operating_Procedure-2023.pdf Standard Operating Procedure]
*[https://wiki.nanofab.ucsb.edu/w/images/3/39/Focus_and_exposure_optimization-_Autostep200-II.pdf Optimizing the Process] - Focus-Exposure Matrix (FEM) instructions
*[[Autostep 200 Troubleshooting and Recovery|Troubleshooting and Recovery]]

===Job Programming===

*[https://wiki.nanofab.ucsb.edu/w/images/2/27/Autostep_200_-_Setting_up_the_Job.pdf Programming a Job] - Detailed instructions
*[[Stepper 2 (Autostep 200) - Job Programming|Programming Differences between Piece-parts and Full Wafers]]

*[https://wiki.nanofab.ucsb.edu/w/images/9/90/5th_draft_Autostep200_Quarter_FIRST_LAYER.pdf Quarter-First Layer Instructions]

*[https://wiki.nanofab.ucsb.edu/w/images/f/f6/Autostep200_Quarter_SECOND_LAYER_.pdf Quarter-Second Layer Instructions]

===Video Training===
These video trainings have bookmarks to skip to specific sections - use them as reference.

Remember, you are NOT authorized to use the system until a [[Biljana Stamenic|supervisor]] grants you access.
*'''[https://gauchocast.hosted.panopto.com/Panopto/Pages/Viewer.aspx?id=a2628454-e507-448a-b363-b29300881115 Video Training for the GCA AutoStep 200]''' on Canvas.

::[[File:GCA Autostep 200 training vid title screen.png|none|thumb|300x300px|link=https://gauchocast.hosted.panopto.com/Panopto/Pages/Viewer.aspx?id=fa7462ce-6f71-49b4-89c4-b20201393f94]]
After studying this video, [https://signupmonkey.ece.ucsb.edu/cgi-bin/users/request-training.cgi?tool_ID=38 request training on SignupMonkey here:]
{{ToolTrainingButton
|toolid = 38
}}

===Reference/Other Info===

*[[Autostep 200 Mask Making Guidance|'''Mask Making Guidelines''']] - ''for designing and ordering photomasks''
*[https://wiki.nanofab.ucsb.edu/w/images/2/2e/Autostep_200_Stepper_manual_focus.pdf Focus Mechanism & Manual Focus] - Info on how the focus system works and how to use Manual Focus effectively. Written by Molly Piels.
*[https://wiki.nanofab.ucsb.edu/w/images/e/e1/AUTOSTEP_200_User_Accessible_Commands_010524.pdf User Accessible Commands]
*[https://wiki.nanofab.ucsb.edu/w/images/5/54/Autostep200_Training_Old_Training_Manual.pdf Training Manual (old version)]

== Recipes ==

* '''[[Stepper Recipes#Stepper 2 (AutoStep 200)|Recipes > Lithography > Stepper Recipes > Stepper #2]]''' - starting processes for various I-Line photoresists, including Dose/Focus values.To calibrate your own Litho processes, you will need to:

* Run your own [https://wiki.nanofab.ucsb.edu/w/images/3/39/Focus_and_exposure_optimization-_Autostep200-II.pdf Focus Exposure Matrix] - instructions for doing this on the AutoStep 200.
* [[Lithography Calibration - Analyzing a Focus-Exposure Matrix]] - how to analyze an FEM

Litho. recipes for all our photolith. tools can be found on the [[Lithography Recipes#Photolithography%20Recipes|Photolithography Recipes]] page.

==Maintenance Procedures==
''These procedures are for Staff / Special use only - contact staff if you think you need to run these!''

*[https://wiki.nanotech.ucsb.edu/w/images/5/5e/Autostep_200_Restart_SOP_June_2021.pdf Shutdown + Startup Procedure]

==Related Tools==

*[[Stepper 1 (GCA 6300)]] - similar tool, compatible photomasks, but with manual photomask alignment and no DFAS. Can't shoot multiple mask plates in single session.

Latest revision as of 04:01, 6 December 2025

Stepper 2 (AutoStep 200)
Location Bay 6
Tool Type Lithography
Manufacturer GCA
Description GCA 200 I-Line Wafer Stepper

Primary Supervisor Biljana Stamenic
(805) 893-4002
biljana@ece.ucsb.edu

Secondary Supervisor

Bill Millerski


Recipes Lithography Recipes

SignupMonkey: Sign up for this tool


Instructions + Procedures

Sign Up

Get Trained

Maintenance
Messages
Report Issue



About

Our GCA wafer stepper is an i-line (365 nm) step and repeat exposure tool for doing lithography that requires high resolution (≥500nm) and/or critical alignment (≥150nm).

The system has been modified to accept piece parts (down to smaller than 10mm x 10mm) up to 6” diameter wafers using manual wafer loading. The maximum square die size is 14.8 mm x 14.8 mm.

The system has an Olympus 2145 (N.A. = 0.45) lens that reduces the mask image by 5x and gives an ultimate resolution of better than 0.5 um in the center of the lens field. The system can easily produce 0.7 um isolated lines across the entire field. The Autostep200 system has 3-point wafer leveling to improve focus uniformity across the field. Autofocus is used to determine the sample surface relative to the lens, making the focus stable and repeatable for different thickness of wafer. The stages are controlled by stepper motors and laser interferometers.

Using the "global", manual alignment, better than 0.25 um alignment error is achievable. Using the DFAS "local" alignment system, alignment error better than 0.15 um is achieved. With the 1000 W Hg arc lamp, we get about 420 mW/cm² of i-line intensity at the wafer.

The system is computer controlled with the capability to program and save a wide variety of exposure jobs. We also have unlimited phone support for system problems through a service contract.


Tutorial: If you are not familiar with the differences between Contact Litho and Stepper Litho, please review this short tutorial: Demis D. John - Stepper_Reticle_Layout_vs_Wafer_Layout.pdf

  • Explains how a Stepper mask can have many designs, and flexibly pattern the wafer with combos of designs.

Detailed Specifications

  • Lens: Olympus 2145: NA = 0.45; Depth of field = 1.2 um for 0.6 um process
  • Maximum die size: ~ 15 mm x 15 mm
  • Maximum substrate thickness: we have various chucks with shims to allow different thicknesses - contact staff for info.
  • Resolution: 400-450 nm for R&D; 700 nm over entire 15 mm x 15 mm field
  • Registration tolerance: 0.25 µm global alignment; Max 0.15 µm local alignment (with care, you can achieve < 0.10 µm registration)
  • Substrate size: ~ 10 x 10 mm up to 100 mm (150 mm possible, we don't provide the vacuum chuck for it).
  • Computer programmable, recipes saved on hard disk
  • Reticle alignment fiducials and global/local fiducials available - contact us for CAD files.
  • Mask Plates: 5x5x0.090 inches, 5x reduction, typically Soda Lime Glass (Quartz is also acceptable), no pellicle.

Process Information

Photomask Info

Recipes

Photoresists

  • The laboratory contains a variety of i-line compatible photoresists. See the Photolith. Recipes Page for detailed processing info (bakes/spins/exposure does etc.). Basic photoresists include:
    • 955CM-0.9 for 0.7-1.0 um thick positive processes.
    • AZ5214E for 1.0 um thick image reversal (negative) process.
    • SPR955CM-1.8 for 1.5-2.0 um thick positive processes.
    • SPR220-3 for 2.5-5 um thick positive process.
    • SPR220-7 for >5 um thick positive processes.
    • AZnLOF5510 for <1.0um and AZnLOF 2020 for 1.5-3 um negative resist process.
    • Shipley LOL-2000 is also used as an underlayer for high resolution lift-off processes.

CAD Files

Service Provider

Operating Procedures

Tool Operation

Job Programming

Video Training

These video trainings have bookmarks to skip to specific sections - use them as reference.

Remember, you are NOT authorized to use the system until a supervisor grants you access.

After studying this video, request training on SignupMonkey here:

Request Training


Reference/Other Info

Recipes

Litho. recipes for all our photolith. tools can be found on the Photolithography Recipes page.

Maintenance Procedures

These procedures are for Staff / Special use only - contact staff if you think you need to run these!

Related Tools

  • Stepper 1 (GCA 6300) - similar tool, compatible photomasks, but with manual photomask alignment and no DFAS. Can't shoot multiple mask plates in single session.