==[[Dicing Saw (ADT)|Dicing Saw Recipes (ADT 7100)]]==
==[[Dicing Saw (ADT)|Dicing Saw Recipes (ADT 7100)]]==

===Dicing Alignment Instructions===
The Process Group often has users fill out these instructions below to fully define a dicing job. This will ensure you have thought about the entire dicing process.

Note that you should design your chips with ≥250µm dicing street width, to avoid the blade cutting into your devices.

It is very helpful to also place alignment guides in the dicing streets, such as crosses at the intersections of dicing streets, such as this:

<code>---- + ---- + ---- + ---</code>

<code>     |      |      |</code>

<code>---- + ---- + ---- + ---</code>

<code>     |      |      |</code>

<code>---- + ---- + ---- + ---</code>

*[https://wiki.nanofab.ucsb.edu/w/images/3/3a/Example_Dicing_Instructions_for_UC_Santa_Barbara_v1.pptx '''Example Dicing Instructions for UC Santa Barbara v1.pptx''']


===Recommended Dicing Parameters===
===Recommended Dicing Parameters===
This table is for our stocked [https://www.dicing.com Thermocarbon] Resnoid blades.
This table is for our stocked [https://www.dicing.com Thermocarbon] Resnoid blades.


-4C blades are 4mils/100µm wide, while -8C blades are 8mils/200µm wide. Plan for ~50–100µm extra edge clearance to account for chipping etc.
-2C blades are 2mils/50µm wide, -4C blades are 4mils/100µm wide, and -8C blades are 8mils/200µm wide. Plan for ~10–30µm extra edge clearance to account for kerf, chipping, etc.


Narrower (~30-50µm) Nickel Hubbed blades are often used for even narrower dicing streets, these must be purchased by the user.
Narrower (~30-50µm) Nickel Hubbed blades are often used for even narrower dicing streets, these must be purchased by the user. KnS G1440-Q5H0 work very well, with ~30µm blade width and smaller kerf. You need to insert a shim to use these blades - please contact [[Dicing Saw (ADT)|tool supervisor]] for how to use these blades.
{| class="wikitable sortable"
{| class="wikitable sortable"
|-
|-
Line 16: Line 35:
!Cut Speed
!Cut Speed
(mm/s)
(mm/s)
!Mohs Hardness
Scale*
|-
|-
|Alumina, AlN
|Alumina, AlN
Line 21: Line 42:
|25
|25
|0.5-2
|0.5-2
|8
|-
|-
|Ceramic
|Ceramic
Line 26: Line 48:
|18
|18
|0.5-2
|0.5-2
|7 - 9
|-
|-
|GaAs
|GaAs
Line 31: Line 54:
|35
|35
|1-5
|1-5
|4.5
|-
|-
|GaN  (<550um)
|GaN  (<550um)
Line 36: Line 60:
|35
|35
|0.5-3
|0.5-3
|9
|-
|-
|GaN  (>550um)
|GaN  (>550um)
Line 41: Line 66:
|35
|35
|0.5-2
|0.5-2
|9
|-
|-
|Glass/Fused Silica
|Glass/Fused Silica
Line 46: Line 72:
|25
|25
|1-5
|1-5
|5.3 - 6.5
|-
|Ga<sub>2</sub>O<sub>3</sub><sup>**</sup>
|2.187-8C-54RU-3
|18
|0.5
|9
|-
|-
|InP
|InP
Line 51: Line 84:
|35
|35
|1-5
|1-5
|9
|-
|-
|Quartz
|Quartz
Line 56: Line 90:
|25
|25
|1-5
|1-5
|7
|-
|-
|Sapphire
|Sapphire<sup>**</sup>
|2.187-8C-54RU-3
|2.187-8C-54RU-3
|18
|18
|0.5-2
|0.5-2
|9
|-
|Si
|2.187-2C-9RU-3
|30
|1-2
|7
|-
|-
|Si
|Si
Line 66: Line 108:
|35
|35
|4-10
|4-10
|7
|-
|-
|Si on Glasss
|Si on Glass
|2.187-4C-9RU-3
|2.187-4C-9RU-3
|25
|25
|1-5
|1-5
|7
|-
|-
|SiC
|SiC
Line 76: Line 120:
|25
|25
|0.5-2
|0.5-2
|9.5
|-
|-
|Ti
|Ti
Line 81: Line 126:
|15
|15
|0.5-2
|0.5-2
|6
|}
|}
<nowiki>*</nowiki> If you do not see the material you want to dice listed, refer to the Mohs Hardness scale for Blade P/N.

<nowiki>**</nowiki> Refer to [[Packaging Recipes#Dual-Pass Dicing|Dual-Pass Dicing]] process below.


====Anatomy of a Blade====
====Anatomy of a Blade====
Example: '''2.187-4C-9RU-3'''
Example: '''2.187-4C-9RU-3'''


"2.187": This is the blade Diameter in inches (55.56mm).
"2.187": This is the blade Outer Diameter ("OD") in inches (55.55 mm).

"4C": Blade thickness in mils. 4 mil = 100 µm


"9": Diamond particle size in microns. Stocked resin blades have embedded diamond particles. Smaller particles create a smoother kerf, but remove less material and are thus less robust or require slower cutting speeds.
"4C": Blade thickness in mils. 4mil = 100µm


"9RU": Diamond particle size in microns. Stocked resin blades have embedded diamond particles. Smaller particles create a smoother kerf, but remove less material and are thus less robust (or require slower cutting speeds) "RU-3" is a blade parameter that deals with cut quality vs. robustness (lifetime) of the blade.
"RU-3". A blade parameter that deals with cut quality vs. robustness (lifetime) of the blade.


===Calculated Blade Exposures===
===Calculated Blade Exposures===
Line 99: Line 150:
!
!
|-
|-
|2.187" (55.55mm)
|2.187" (55.55 mm)
|47 mm
|47mm
|4.275mm
|4.275 mm
|
|
|-
|-
|2.187" (55.55mm)
|2.187" (55.55 mm)
|49 mm
|49mm
|3.275mm
|3.275 mm
|
|
|-
|-
|2.187" (55.55mm)
|2.187" (55.55 mm)
|51 mm
|51mm
|2.275mm
|2.275 mm
|
|''51mm Currently Unavailable''
|-
|-
|2.187" (55.55mm)
|2.187" (55.55 mm)
|52 mm
|52mm
|1.775mm
|1.775 mm
|
|
|-
|-
|2.187" (55.55mm)
|2.187" (55.55 mm)
|53 mm
|53mm
|1.275mm
|1.275 mm
|
|
|}
|}


====Blade Exposure Calculation====
====Blade Exposure Calculation====
[[File:ADT Dicing - Blade Exposure diagram.png|alt=schematic of blade exposure|none|thumb|388x388px|Diagram of blade exposure]]
[[File:ADT Dicing - Blade Exposure diagram.png|alt=schematic of blade exposure|none|thumb|600x600px|Diagram of blade exposure. If '''''A''''' '''''< 0.30mm''''', then the flange may hit your wafer, damaging the tool and wafer!]]


===Mounting/Unmounting Samples===
===Mounting/Unmounting Samples===
The UV-Release Tape dispenser is most-often used for mounting sample for dicing.
The UV-Release Tape dispenser is most-often used for mounting sample for dicing.


The Tape Model installed is Ultron 1042R. [[ADT_UV-Tape_Table_1042R|Data Sheet Here]].
The Tape Model installed is Ultron 1042R-B. [https://wiki.nanofab.ucsb.edu/w/images/a/ac/Ultron_1042R-B_Film_Specs.pdf Data Sheet Here.]


*[[ADT WM-966 - UV Tape Mounting Standard Procedure|Procedure for mounting sample on UV-Release Tape]]
*[[ADT WM-966 - UV Tape Mounting Standard Procedure|Procedure for mounting sample on UV-Release Tape]]
*Full Release: 60 sec exposure
*Full Release: 120 sec exposure
*Partial Release for Shipping: 9 sec exposure
*Partial Release for Shipping: 9 sec exposure

====Wax-Mounting to Carrier====
If your final die size will be very small, eg. <3mm square or so, the chances increase that many die will be ejected into the cooling water stream once you begin the 2nd cut angle, because the total surface area of die contacting the adhesive tape becomes very low

A method to overcome this is to mount your sample with CrystalBond wax onto a Silicon carrier wafer. The wax is a much stronger adhesive. The drawback is that you must dissolve the wax to unmount your die, often resulting in a jumbled pile of small die in Acetone/Isopropanol, which can be difficult to handle/sort afterwards.

<br />
{| class="wikitable"
|+
!Procedure to mount with wax onto a carrier wafer:
|-
|
* Prepare a clean silicon carrier wafers, at least ~5mm larger than your sample to be diced.
* The Bay 5 solvent bench is most commonly used for wax mounting, although any solvent bench can be used as long as you cover the hotplate with wax and are careful to clean up any mess.
* Cover the hotplate (cool) with clean tinfoil, and then raise temp to 130-150°C.
* Place the silicon carrier on top, polished wide up, and wait a few min for it to heat up. Pressing down with tweezers can help speed this up.
* Take either a small measured/weighed piece of crystalbond wax, or the whole stick, and touch/press it against the silicon carrier. The wax sticks are stored often on the bench shelves, edge of the bench, or the outside wall of the bench (where the vacuum ports are for the Bay 4 solvent bench).
* Once a large enough puddle of melted wax is produced, remove the wax stick (use tweezers to hold the carrier wafer down), being careful to prevent the wax stringers from landing all over the workspace. You can clean it up later when the hotplate is cold.
** You want to make sure the entire underside of the sample will be contacting the wax, but don’t want so much wax that the sample will be tilted/uneven. Excess wax can easily be removed on an upcoming step.
* With tweezers, place your sample to be diced on the wax, face up.
* Optional: press down the edges/corners of the sample to make it approximately flat.
* Remove the entire tinfoil sheet, with carrier wafer, from the hotplate to let it cool down. Once cool (few mins), remove your silicon carrier with sample attached.
* Optional: To remove wax from the top surface of your sample, or from the edges, one effective way is to place the mounted assembly onto a POLOS spinner and, while spinning at ~1500-2000rpm, spray with ACE spray bottle for ~30sec, the ISO & N2 dry. This removes wax on the top without significantly attacking the wax mounting between the samples. You could also attempt to use a cotton swab with ACE, although this is typically much less clean.
* Proceed to apply your surface protection for dicing, eg. Photoresist coating or blue tape etc.
|-
|''Procedure written by Demis D John, 2022-07-04. Please consider the [https://wiki.nanotech.ucsb.edu/wiki/Frequently_Asked_Questions#Publications_acknowledging_the_Nanofab publication policy].''
|}
<br />


===Dicing Tips===
===Dicing Tips===
Line 157: Line 236:
#Perform your dicing
#Perform your dicing
#Remove the die from the UV release tape (60sec UV Exposure)
#Remove the die from the UV release tape (60sec UV Exposure)
#Strip the PR from each die in Acetone and ISO & N2 dry
#Strip the PR from each die in Acetone and ISO & N2 dry. We recommend to use ACE/ISO squirt bottles on each die individually to ensure the particles on the PR surface don’t land and stick to the chip surface.


====Blue Tape====
====Blue Tape====
Alternatively our low-tack residue-free Blue tape can be used to protect the die surface. Blue tape removal is easy for large die, but does require manual removal from each die, and eliminates sample exposure to solvents.
Alternatively our low-tack residue-free Blue tape can be used to protect the die surface.

Blue tape removal is easy for large die, but does require manual removal from each die, and eliminates sample exposure to solvents.

You will need to physically, gently press the blue tape onto the wafer surface, while eliminating bubbles. Do this by placing your wafer directly in front of the blue tape-roll dispenser, then attaching the tape to the table over the wafer (without touching wafer), allowing you to press the tape onto the wafer progressively from one side.


The very edges of the die may accumulate a bit more dicing dust due to the tape delaminating slightly during dicing. Plan for about 50-100µm of edge clearance on each die.
The very edges of the die may accumulate a bit more dicing dust due to the tape delaminating slightly during dicing. Plan for about 50-100µm of edge clearance on each die.

=== Cut Depth Accuracy ===
Depth accuracy (distance between bottom of the blade and sample chuck) (a) is only accurate to ~20µm or so, and (b) varies by at least~10µm across the chuck. If you need to leave a certain amount of your substrate uncut, here is a way to improve the accuracy, adds ~30-60min to your process.

==== Procedure to improve cut depth accuracy ====
To achieve an accurate depth like <30µm accuracy:

* Do Manual alignment of sample.
* You will do test cuts on the tape only (with sample mounted, but ~50mm away from sample in Y-direction (not X!)) - nominally 90µm thick but I think the plastic thickness varies between ~60-100µm as a guess. Then progressively reduce the depth to se when it hits the tape.  
* Do Manual y-offset, with depth (distance between tip of blade & chuck)=0.070mm
* If you don’t see a cut, then [Cancel]
* Adjust recipe to -0.010mm depth, 0.060mm in this case
* Do Manual Y-offset again 10mm away from original cut
* Repeat until you see the blade just scraping the surface.  You will see it “skips”, hitting then missing then hitting (this is the tape or chuck height variation)
** That is the depth to hit the tape.
* (To ascertain the variation, keep going down by 10µm increments until you see a “full” cut with no skips.)
* Then in your recipe, add the desired remaining amount
** eg. Depth to hit tape = 0.060mm + 0.070mm remaining uncut sample = 0.130mm cut depth.  
** (30µm will also work, you’ll just see it varies by ~20µm across the cut.)

=== Dual-Pass Dicing ===
For hard (≥ 9 Mohs Hardness) wafers thicker than 400µm or so, you likely need to do double-pass dicing, where you cut 1/2 of the thickness the first pass, then cut the full wafer thickness on the second pass. Setting up the recipe:

1. Setup: Enter wafer thickness (for example:660um), and tape thickness (100um)

2. Cut:

* Index "0" - Set this to desired index (distance between two cuts), index "1" - set this to "0"
* Cut: Depth - Head1 "0"- set this to half way of actual thickness, for example: 0.300mm
* Cut: Depth - Head1 "1"- set this to cut the full thickness (wafer + cutting 20-30um into tape), for example: 0.070mm

3. Height: Check it after every cut

4. Example of dicing different materials:

a) Very thick Ga<sub>2</sub>O<sub>3</sub> (660um), used double pass, blade 2.187-8C-54RU-3, expected kerf ~(210-230)um, actual kerf ~225um

b) Very thick Sapphire (650um), used double pass, blade 2.187-8C-54RU-3, kerf ~(210-230)um, actual kerf ~240um

5. Recipe example for Dual Dicing and Kerf for Ga<sub>2</sub>O<sub>3</sub>

<gallery>
File:Dicing Thick Ga2O3.jpg|Recipe example for Dicing Ga<sub>2</sub>O<sub>3</sub>
File:Kerf 225um 660um thick Ga2O3 dual pass.png|Measured kerf for Ga<sub>2</sub>O<sub>3</sub> (with photoresist on surface)
</gallery>
Author: [[Biljana Stamenic]], 2026-06

=== Partial Dicing ===
For partial-depth dicing, you need to do single-pass, dicing into substrate desired depth. Setting up the recipe:

1. Setup: Enter wafer thickness (example:750um), and tape (90um)

2. Cut: (if partial cut is only 100um- looking from top of the substrate)

* Index "0" - Set this to desired index (distance between two cuts, for example: 0.105mm), index "1" - set this to "0"
* Cut: Depth - Head1 "1"- Set Depth as following [(wafer thickness + tape thickness)- partial cut depth]=(750+90)-100=740um

3. Height: Check height after every 5 cuts

4. Example of partial cut:

a) Very thick Si (750um), used single pass, blade 2.187-2C-9RU-3, cutting speed=0.5mm/sec, spindle speed=30KRPM

5. Recipe example for Partial dicing into Si substrate
[[File:Partial dicing.jpeg|thumb|150x150px|none|Cut parameters for partial-depth cut]]
Author: [[Biljana Stamenic]], 2026-06


==[[Wafer Bonder (Logitech WBS7)]]==
==[[Wafer Bonder (Logitech WBS7)]]==
This tool is used for bonding samples to Silicon carrier wafers with CrystalBond wax.
This tool is used for bonding samples to Silicon carrier wafers with CrystalBond wax.


*[[Logitech WBS7 - Procedure for Wax Mounting with bulk Crystalbond Stick|Wax Mounting Procedure, with bulk Crystalbond Wax]]
*[[Logitech WBS7 - Procedure for Wax Mounting with bulk Crystalbond Stick|Wax Mounting Procedure, with bulk Crystalbond Wax]] - Recommended, works for most applications.
*[[Logitech WBS7 - Procedure for Wax Mounting with Spin-On Crystalbond|Wax Mounting Procedure, with Spin-On Crystalbond]]
*[[Logitech WBS7 - Procedure for Wax Mounting with Spin-On Crystalbond|Wax Mounting Procedure, with Spin-On Crystalbond]] - if very thin/high uniformity (≤5µm) is required.

==[[Automated Wafer Cleaver (Loomis LSD-155LT)]]==
This tool is used for scribe and break of your samples.

*Recommended recipes, a starting point for most applications.
*


{| class="wikitable"
{| class="wikitable"

Latest revision as of 22:41, 11 June 2026

Dicing Saw Recipes (ADT 7100)

Dicing Alignment Instructions

The Process Group often has users fill out these instructions below to fully define a dicing job. This will ensure you have thought about the entire dicing process.

Note that you should design your chips with ≥250µm dicing street width, to avoid the blade cutting into your devices.

It is very helpful to also place alignment guides in the dicing streets, such as crosses at the intersections of dicing streets, such as this:

---- + ---- + ---- + ---

     |      |      |

---- + ---- + ---- + ---

     |      |      |

---- + ---- + ---- + ---

Recommended Dicing Parameters

This table is for our stocked Thermocarbon Resnoid blades.

-2C blades are 2mils/50µm wide, -4C blades are 4mils/100µm wide, and -8C blades are 8mils/200µm wide. Plan for ~10–30µm extra edge clearance to account for kerf, chipping, etc.

Narrower (~30-50µm) Nickel Hubbed blades are often used for even narrower dicing streets, these must be purchased by the user. KnS G1440-Q5H0 work very well, with ~30µm blade width and smaller kerf. You need to insert a shim to use these blades - please contact tool supervisor for how to use these blades.

Material Blade P/N Spindle Speed

(KRPM)

Cut Speed

(mm/s)

Mohs Hardness

Scale*

Alumina, AlN 2.187-8C-54RU-3 25 0.5-2 8
Ceramic 2.187-4C-30RU-3 18 0.5-2 7 - 9
GaAs 2.187-4C-9RU-3 35 1-5 4.5
GaN  (<550um) 2.187-4C-30RU-3 35 0.5-3 9
GaN  (>550um) 2.187-8C-30RU-3 35 0.5-2 9
Glass/Fused Silica 2.187-4C-22RU-3 25 1-5 5.3 - 6.5
Ga2O3** 2.187-8C-54RU-3 18 0.5 9
InP 2.187-4C-9RU-3 35 1-5 9
Quartz 2.187-4C-30RU-3 25 1-5 7
Sapphire** 2.187-8C-54RU-3 18 0.5-2 9
Si 2.187-2C-9RU-3 30 1-2 7
Si 2.187-4C-9RU-3 35 4-10 7
Si on Glass 2.187-4C-9RU-3 25 1-5 7
SiC 2.187-8C-30RU-3 25 0.5-2 9.5
Ti 2.187-8C-54RU-3 15 0.5-2 6

* If you do not see the material you want to dice listed, refer to the Mohs Hardness scale for Blade P/N.

** Refer to Dual-Pass Dicing process below.

Anatomy of a Blade

Example: 2.187-4C-9RU-3

"2.187": This is the blade Outer Diameter ("OD") in inches (55.55 mm).

"4C": Blade thickness in mils. 4 mil = 100 µm

"9": Diamond particle size in microns. Stocked resin blades have embedded diamond particles. Smaller particles create a smoother kerf, but remove less material and are thus less robust or require slower cutting speeds.

"RU-3". A blade parameter that deals with cut quality vs. robustness (lifetime) of the blade.

Calculated Blade Exposures

Blade Diam Flange Diam. Blade Exposure
2.187" (55.55 mm) 47 mm 4.275 mm
2.187" (55.55 mm) 49 mm 3.275 mm
2.187" (55.55 mm) 51 mm 2.275 mm
2.187" (55.55 mm) 52 mm 1.775 mm
2.187" (55.55 mm) 53 mm 1.275 mm

Blade Exposure Calculation

schematic of blade exposure
Diagram of blade exposure. If A < 0.30mm, then the flange may hit your wafer, damaging the tool and wafer!

Mounting/Unmounting Samples

The UV-Release Tape dispenser is most-often used for mounting sample for dicing.

The Tape Model installed is Ultron 1042R-B. Data Sheet Here.

Wax-Mounting to Carrier

If your final die size will be very small, eg. <3mm square or so, the chances increase that many die will be ejected into the cooling water stream once you begin the 2nd cut angle, because the total surface area of die contacting the adhesive tape becomes very low

A method to overcome this is to mount your sample with CrystalBond wax onto a Silicon carrier wafer. The wax is a much stronger adhesive. The drawback is that you must dissolve the wax to unmount your die, often resulting in a jumbled pile of small die in Acetone/Isopropanol, which can be difficult to handle/sort afterwards.


Procedure to mount with wax onto a carrier wafer:
  • Prepare a clean silicon carrier wafers, at least ~5mm larger than your sample to be diced.
  • The Bay 5 solvent bench is most commonly used for wax mounting, although any solvent bench can be used as long as you cover the hotplate with wax and are careful to clean up any mess.
  • Cover the hotplate (cool) with clean tinfoil, and then raise temp to 130-150°C.
  • Place the silicon carrier on top, polished wide up, and wait a few min for it to heat up. Pressing down with tweezers can help speed this up.
  • Take either a small measured/weighed piece of crystalbond wax, or the whole stick, and touch/press it against the silicon carrier. The wax sticks are stored often on the bench shelves, edge of the bench, or the outside wall of the bench (where the vacuum ports are for the Bay 4 solvent bench).
  • Once a large enough puddle of melted wax is produced, remove the wax stick (use tweezers to hold the carrier wafer down), being careful to prevent the wax stringers from landing all over the workspace. You can clean it up later when the hotplate is cold.
    • You want to make sure the entire underside of the sample will be contacting the wax, but don’t want so much wax that the sample will be tilted/uneven. Excess wax can easily be removed on an upcoming step.
  • With tweezers, place your sample to be diced on the wax, face up.
  • Optional: press down the edges/corners of the sample to make it approximately flat.
  • Remove the entire tinfoil sheet, with carrier wafer, from the hotplate to let it cool down. Once cool (few mins), remove your silicon carrier with sample attached.
  • Optional: To remove wax from the top surface of your sample, or from the edges, one effective way is to place the mounted assembly onto a POLOS spinner and, while spinning at ~1500-2000rpm, spray with ACE spray bottle for ~30sec, the ISO & N2 dry. This removes wax on the top without significantly attacking the wax mounting between the samples. You could also attempt to use a cotton swab with ACE, although this is typically much less clean.
  • Proceed to apply your surface protection for dicing, eg. Photoresist coating or blue tape etc.
Procedure written by Demis D John, 2022-07-04. Please consider the publication policy.


Dicing Tips

Harder materials will often require larger diamond particle sizes, and thicker blades will last longer if they are overheating and breaking often.

It is not uncommon to have to change a blade in the middle of cutting a wafer - the software is set up to allow this easily without aborting the programmed cuts. The "Height Check Rate" in the recipe will check the blade exposure after this many cuts, using the optical height sensor - this allows you to see how quickly the blade is wearing out (as blade exposure reduces).

Ensuring the cut water jet is hitting at ~7-8 o'clock on the blade and the water jet is being split in two will keep the blade coolest and help prevent breakage. Water sprays should be set to 0.9/0.9/0.9 by default.

For sapphire dicing (very hard material), it is common to use "double-pass dicing", where the substrate is cut at only half depth (eg. cutting only 150µm deep for a 300µm thick substrate) on the first pass, and then re-cut at the full depth. The blade will need to be changed often, so set your "Height Check Rate" to 1 or 2. This can be very time consuming. 200-300µm thick Sapphire substrates are much easier to cut than 650µm thick - often single-pass dicing is adequate for the thinner substrates.

Surface Protection

Photoresist

Users most often use sacrificial photoresists to protect the surface from accumulating dicing dust. The static-buildup of dielectric films causes the dust to adhere strongly. Ensure that the PR thickness will adequately coat all your exposed topography (eg. use a ≥2µm thick PR for protecting 1.5-2.0µm tall etched features).

  1. Choose a photoresist of appropriate thickness, and spin-coat it & soft-bake it according to a standard recipe.
    1. Contact Alignment PR Recipes
    2. Stepper PR Recipes
  1. Perform your dicing
  2. Remove the die from the UV release tape (60sec UV Exposure)
  3. Strip the PR from each die in Acetone and ISO & N2 dry. We recommend to use ACE/ISO squirt bottles on each die individually to ensure the particles on the PR surface don’t land and stick to the chip surface.

Blue Tape

Alternatively our low-tack residue-free Blue tape can be used to protect the die surface.

Blue tape removal is easy for large die, but does require manual removal from each die, and eliminates sample exposure to solvents.

You will need to physically, gently press the blue tape onto the wafer surface, while eliminating bubbles. Do this by placing your wafer directly in front of the blue tape-roll dispenser, then attaching the tape to the table over the wafer (without touching wafer), allowing you to press the tape onto the wafer progressively from one side.

The very edges of the die may accumulate a bit more dicing dust due to the tape delaminating slightly during dicing. Plan for about 50-100µm of edge clearance on each die.

Cut Depth Accuracy

Depth accuracy (distance between bottom of the blade and sample chuck) (a) is only accurate to ~20µm or so, and (b) varies by at least~10µm across the chuck. If you need to leave a certain amount of your substrate uncut, here is a way to improve the accuracy, adds ~30-60min to your process.

Procedure to improve cut depth accuracy

To achieve an accurate depth like <30µm accuracy:

  • Do Manual alignment of sample.
  • You will do test cuts on the tape only (with sample mounted, but ~50mm away from sample in Y-direction (not X!)) - nominally 90µm thick but I think the plastic thickness varies between ~60-100µm as a guess. Then progressively reduce the depth to se when it hits the tape.  
  • Do Manual y-offset, with depth (distance between tip of blade & chuck)=0.070mm
  • If you don’t see a cut, then [Cancel]
  • Adjust recipe to -0.010mm depth, 0.060mm in this case
  • Do Manual Y-offset again 10mm away from original cut
  • Repeat until you see the blade just scraping the surface.  You will see it “skips”, hitting then missing then hitting (this is the tape or chuck height variation)
    • That is the depth to hit the tape.
  • (To ascertain the variation, keep going down by 10µm increments until you see a “full” cut with no skips.)
  • Then in your recipe, add the desired remaining amount
    • eg. Depth to hit tape = 0.060mm + 0.070mm remaining uncut sample = 0.130mm cut depth.  
    • (30µm will also work, you’ll just see it varies by ~20µm across the cut.)

Dual-Pass Dicing

For hard (≥ 9 Mohs Hardness) wafers thicker than 400µm or so, you likely need to do double-pass dicing, where you cut 1/2 of the thickness the first pass, then cut the full wafer thickness on the second pass. Setting up the recipe:

1. Setup: Enter wafer thickness (for example:660um), and tape thickness (100um)

2. Cut:

  • Index "0" - Set this to desired index (distance between two cuts), index "1" - set this to "0"
  • Cut: Depth - Head1 "0"- set this to half way of actual thickness, for example: 0.300mm
  • Cut: Depth - Head1 "1"- set this to cut the full thickness (wafer + cutting 20-30um into tape), for example: 0.070mm

3. Height: Check it after every cut

4. Example of dicing different materials:

a) Very thick Ga2O3 (660um), used double pass, blade 2.187-8C-54RU-3, expected kerf ~(210-230)um, actual kerf ~225um

b) Very thick Sapphire (650um), used double pass, blade 2.187-8C-54RU-3, kerf ~(210-230)um, actual kerf ~240um

5. Recipe example for Dual Dicing and Kerf for Ga2O3

Author: Biljana Stamenic, 2026-06

Partial Dicing

For partial-depth dicing, you need to do single-pass, dicing into substrate desired depth. Setting up the recipe:

1. Setup: Enter wafer thickness (example:750um), and tape (90um)

2. Cut: (if partial cut is only 100um- looking from top of the substrate)

  • Index "0" - Set this to desired index (distance between two cuts, for example: 0.105mm), index "1" - set this to "0"
  • Cut: Depth - Head1 "1"- Set Depth as following [(wafer thickness + tape thickness)- partial cut depth]=(750+90)-100=740um

3. Height: Check height after every 5 cuts

4. Example of partial cut:

a) Very thick Si (750um), used single pass, blade 2.187-2C-9RU-3, cutting speed=0.5mm/sec, spindle speed=30KRPM

5. Recipe example for Partial dicing into Si substrate

Cut parameters for partial-depth cut
Author: Biljana Stamenic, 2026-06

Wafer Bonder (Logitech WBS7)

This tool is used for bonding samples to Silicon carrier wafers with CrystalBond wax.

Automated Wafer Cleaver (Loomis LSD-155LT)

This tool is used for scribe and break of your samples.

  • Recommended recipes, a starting point for most applications.