=== Thermal Oxidation of Silicon - Calculating Oxidation Times ===
===Thermal Oxidation of Silicon - Calculating Oxidation Times===
Online calculators for thermal oxidation can be used to estimate the oxidation time for a desired oxidation thickness.
Online calculators for thermal oxidation can be used to estimate the oxidation time for a desired oxidation thickness.
Please see the [[Calculators + Utilities]] page for links to these oxidation calculators.
Please see the [[Calculators + Utilities]] page for links to these oxidation calculators.
Line 7: Line 7:
Using the [http://www.lelandstanfordjunior.com/thermaloxide.html Stanford Leland Jr. "Advanced Silicon Thermal Oxide Thickness Calculator"], we have determined the following simulation parameters (“partial pressure” in particular) to predict oxidation times. Please note, however, that doping level, impurity concentration and other factors can alter these calibrations, so you may need to calibrate the ''Partial Pressure'' yourself if you need higher accuracy.
Using the [http://www.lelandstanfordjunior.com/thermaloxide.html Stanford Leland Jr. "Advanced Silicon Thermal Oxide Thickness Calculator"], we have determined the following simulation parameters (“partial pressure” in particular) to predict oxidation times. Please note, however, that doping level, impurity concentration and other factors can alter these calibrations, so you may need to calibrate the ''Partial Pressure'' yourself if you need higher accuracy.


=== Thermal Oxidation Recipes ===
===Thermal Oxidation Recipes===


==== 1050°C Dry Oxidation ====
====1050°C Dry Oxidation====

* Recipe Name: '''''DRY1050'''''
*Recipe Name: '''''DRY1050'''''
* Tube #2 for Cleaned Silicon Only
* Tube #3 for processed silicon or other anneals.
*Tube #2 for Cleaned Silicon Only
*Tube #3 for processed silicon or other anneals.

⚫
=====Simulation Parameters=====

⚫
*Partial Pressure = 1.12 (best fit to measured data below)
⚫
*<100>, 1050°C, 10Å Native Oxide, no dopants


⚫
===== Simulation Parameters =====
⚫
* Partial Pressure = 1.12 (best fit to measured data below)
⚫
* <100>, 1050°C, 10Å Native Oxide, no dopants
[[File:TyStar_Thermal_Oxidations_-_DryOx_1050°C_2018-04-09.png|alt=plot of Measurements and Curve-Fitting for 1050°C Dry oxidations.|none|thumb|300x300px|'''Measurements and Curve-Fitting for 1050°C Dry oxidations. Note: three data points only. ''(Demis D. John, 2017-12)''''']]
[[File:TyStar_Thermal_Oxidations_-_DryOx_1050°C_2018-04-09.png|alt=plot of Measurements and Curve-Fitting for 1050°C Dry oxidations.|none|thumb|300x300px|'''Measurements and Curve-Fitting for 1050°C Dry oxidations. Note: three data points only. ''(Demis D. John, 2017-12)''''']]


==== 1050°C Wet Oxidation ====
====1050°C Wet Oxidation====

* Recipe Name: '''''WET1050'''''
*Recipe Name: '''''WET1050'''''
* Tube #2 for Cleaned Silicon Only
* Tube #3 for processed silicon or other anneals.
*Tube #2 for Cleaned Silicon Only
*Tube #3 for processed silicon or other anneals.

⚫
=====Simulation Parameters=====

⚫
*Partial Pressure = 1.09 (best fit to measured data below)
⚫
*<100>, 1050°C, 10Å Native Oxide, no dopants


⚫
===== Simulation Parameters =====
⚫
* Partial Pressure = 1.09 (best fit to measured data below)
⚫
* <100>, 1050°C, 10Å Native Oxide, no dopants
{|
{|
![[File:TyStar_Thermal_Oxidations_-_WetOx_1050°C_2018-04-09.png|alt=plot of Measurements and Curve-Fitting for 1050°C Wet oxidations.|none|thumb|300x300px|Measurements and Curve-Fitting for 1050°C Wet oxidations. '''''(Demis D. John, 2017-12)''''']]
![[File:TyStar_Thermal_Oxidations_-_WetOx_1050°C_2018-04-09.png|alt=plot of Measurements and Curve-Fitting for 1050°C Wet oxidations.|none|thumb|300x300px|Measurements and Curve-Fitting for 1050°C Wet oxidations. '''''(Demis D. John, 2017-12)''''']]
Line 32: Line 38:
|}
|}


==== AlGaAs Oxidation ====
====AlGaAs Oxidation====
A recipe is available on Tube #1 for thermal oxidation of AlGaAs layers, at much lower temperatures than Tubes #2 & #3. There are special procedures for running this lower-temp. oxidation at shorter times, please contact [[Tony Bosch]] or the NanoFab process Group for more information.
A recipe is available on Tube #1 for thermal oxidation of AlGaAs layers, at much lower temperatures than Tubes #2 & #3. There are special procedures for running this lower-temp. oxidation at shorter times, please contact [[Tony Bosch]] or the NanoFab process Group for more information.


==Wafer Substrate Bonding==
==Wafer Substrate Bonding==


=== Direct Bonding ===
===Direct Bonding===
Numerous research groups perform direct wafer bonding (of various materials) using either the [[Wafer Bonder (SUSS SB6-8E)|Suss Wafer Bonder]], or a custom graphite fixture in conjunction with any one of [[Thermal Processing|numerous ovens]], such as the N2-purged [[Tube Furnace Wafer Bonding (Thermco)|Wafer Bonding Furnace]] (with glove box) or N2-purged [[High Temp Oven (Blue M)|Blue M oven]] or HeraTherm oven.
Numerous research groups perform direct wafer bonding (of various materials) using either the [[Wafer Bonder (SUSS SB6-8E)|Suss Wafer Bonder]], or a custom graphite fixture in conjunction with any one of [[Thermal Processing|numerous ovens]], such as the N2-purged [[Tube Furnace Wafer Bonding (Thermco)|Wafer Bonding Furnace]] (with glove box) or N2-purged [[High Temp Oven (Blue M)|Blue M oven]] or HeraTherm oven.


Line 44: Line 50:
The [[Plasma Activation (EVG 810)|EVG Plasma Activation]] system and [[Goniometer (Rame-Hart A-100)|Goniometer]] allow for surface prep/inspection prior to bonding.
The [[Plasma Activation (EVG 810)|EVG Plasma Activation]] system and [[Goniometer (Rame-Hart A-100)|Goniometer]] allow for surface prep/inspection prior to bonding.


=== Bonding with Intermediate layer ===
===Bonding with Intermediate/adhesive layer===
The [[Wafer Bonder (Logitech WBS7)|Logitech Bonder]] allows wafer-bonding with a CrystalBond wax intermediate layer. Please see [[Don Freeborn]] for recipes.
The [[Wafer Bonder (Logitech WBS7)|Logitech Bonder]] allows wafer-bonding with a CrystalBond wax or other intermediate layer, while applying pressure to the top surface to improve uniform wax distribution. Please see the '''''Recipes > Packaging > [[Packaging Recipes#Wafer Bonder .28Logitech WBS7.29|<u>Logitech Bonder</u>]]''''' page for recipes.


== [[Tube Furnace AlGaAs Oxidation (Lindberg)]] ==
==[[Tube Furnace AlGaAs Oxidation (Lindberg)]]==
Oxidation of AlGaAs (high-Aluminum content >90%) is performed in this furnace, at temperatures between 200°C → 500°C.
Oxidation of AlGaAs (high-Aluminum content >90%) is performed in this furnace, at temperatures between 200°C → 500°C.


Line 54: Line 60:
Recipes are available, please ask the NanoFab Process group staff.
Recipes are available, please ask the NanoFab Process group staff.


== [[Rapid Thermal Processor (SSI Solaris 150)]] ==
==[[Rapid Thermal Processor (SSI Solaris 150)]]==
[[Category:Processing]]
[[Category:Processing]]
{{todo|Add starting recipes for RTP}}
{{todo|Add starting recipes for RTP}}

Revision as of 06:14, 20 April 2022

Tystar 8300

Thermal Oxidation of Silicon - Calculating Oxidation Times

Online calculators for thermal oxidation can be used to estimate the oxidation time for a desired oxidation thickness. Please see the Calculators + Utilities page for links to these oxidation calculators.

Using the Stanford Leland Jr. "Advanced Silicon Thermal Oxide Thickness Calculator", we have determined the following simulation parameters (“partial pressure” in particular) to predict oxidation times. Please note, however, that doping level, impurity concentration and other factors can alter these calibrations, so you may need to calibrate the Partial Pressure yourself if you need higher accuracy.

Thermal Oxidation Recipes

1050°C Dry Oxidation

  • Recipe Name: DRY1050
  • Tube #2 for Cleaned Silicon Only
  • Tube #3 for processed silicon or other anneals.
Simulation Parameters
  • Partial Pressure = 1.12 (best fit to measured data below)
  • <100>, 1050°C, 10Å Native Oxide, no dopants
plot of Measurements and Curve-Fitting for 1050°C Dry oxidations.
Measurements and Curve-Fitting for 1050°C Dry oxidations. Note: three data points only. (Demis D. John, 2017-12)

1050°C Wet Oxidation

  • Recipe Name: WET1050
  • Tube #2 for Cleaned Silicon Only
  • Tube #3 for processed silicon or other anneals.
Simulation Parameters
  • Partial Pressure = 1.09 (best fit to measured data below)
  • <100>, 1050°C, 10Å Native Oxide, no dopants
plot of Measurements and Curve-Fitting for 1050°C Wet oxidations.
Measurements and Curve-Fitting for 1050°C Wet oxidations. (Demis D. John, 2017-12)
plot of Zoom-in on Measurements and Curve-Fitting for 1050°C Wet oxidations.
Zoom-in on Measurements and Curve-Fitting for 1050°C Wet oxidations.

AlGaAs Oxidation

A recipe is available on Tube #1 for thermal oxidation of AlGaAs layers, at much lower temperatures than Tubes #2 & #3. There are special procedures for running this lower-temp. oxidation at shorter times, please contact Tony Bosch or the NanoFab process Group for more information.

Wafer Substrate Bonding

Direct Bonding

Numerous research groups perform direct wafer bonding (of various materials) using either the Suss Wafer Bonder, or a custom graphite fixture in conjunction with any one of numerous ovens, such as the N2-purged Wafer Bonding Furnace (with glove box) or N2-purged Blue M oven or HeraTherm oven.

Il addition, the Fine-Tech Flip-Chip Bonder can perform aligned bonding of various-sized pieces. The Fine-Tech can do metal-to-metal thermo-compression bonding with ultrasonic assist.

The EVG Plasma Activation system and Goniometer allow for surface prep/inspection prior to bonding.

Bonding with Intermediate/adhesive layer

The Logitech Bonder allows wafer-bonding with a CrystalBond wax or other intermediate layer, while applying pressure to the top surface to improve uniform wax distribution. Please see the Recipes > Packaging > Logitech Bonder page for recipes.

Tube Furnace AlGaAs Oxidation (Lindberg)

Oxidation of AlGaAs (high-Aluminum content >90%) is performed in this furnace, at temperatures between 200°C → 500°C.

Maximum time is about 3 hours before the bubbler water temperature becomes uncontrolled.

Recipes are available, please ask the NanoFab Process group staff.

Rapid Thermal Processor (SSI Solaris 150)