Direct-Write Lithography Recipes: Difference between revisions
m →Greyscale Lithography: added model to header title |
→E-Beam Lithography Recipes (Raith EBPG 5150+): added alignmetn mark shape |
||
| (71 intermediate revisions by 3 users not shown) | |||
| Line 1: | Line 1: | ||
[[category: Lithography]] |
[[category: Lithography]] |
||
[[category: Recipes]] |
[[category: Recipes]] |
||
{{WIP}} |
|||
__TOC__ |
__TOC__ |
||
== |
==[[Maskless Aligner (Heidelberg MLA150)]]== |
||
For CAD design tips and requirements, see these pages: |
|||
Photolithography Recipes for the [[Maskless Aligner (Heidelberg MLA150)|Heidelberg MLA150]]. ''Description of litho params- different lasers available, greyscale etc.'' |
|||
*[[MLA150 - Design Guidelines|Design Guidelines + Tips]] - ''useful info for designing your CAD files, alignment marks etc.'' |
|||
=== Positive Resist (MLA150) === |
|||
*[[MLA150 - CAD Files and Templates|CAD Files and Templates]] - example CAD files etc. |
|||
''General notes: Hotplates used, filters, laser wavelengths, etc.'' |
|||
Photolithography Recipes for the [[Maskless Aligner (Heidelberg MLA150)|Heidelberg MLA150]]. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point. |
|||
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
These recipes use the same spin and bake params as our contact aligner and stepper recipes, using built-in hotplates on the photoresist spinner benches. |
|||
'''''Any I-Line PR is usable''''', although we only characterized a select few below. Run your own Focus-Exposure Matrix to characterize a new PR. |
|||
'''<u>Note:</u>''' On this tool, it is common to have to run a Focus-Exposure Matrix (aka. FEM), via "''Series''" exposure mode, for each new layer structure and/or critical feature size. The layer structure can strongly affect the exposure parameters. See the [[ASML Stepper 3 Standard Operating Procedure#Tips for FEM analysis|FEM Analysis Tips page]] for how to choose the proper exposure parameters. |
|||
The [[MLA150 - Troubleshooting#Out Of Focus Exposures|'''MLA''' '''Troubleshooting > Out-of-Focus Exposures''']] section can help you avoid bad exposures, please read it! |
|||
===Positive Resist (MLA150)=== |
|||
''We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies; compensate for widening/narrowing using CD Bias [[MLA150 - Design Guidelines#High-Resolution Writing|as described here]].'' |
|||
Note: calibrations done with the "HIMT design" will show higher dose, due to using only dark-field line/space patterns. |
|||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
|||
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
! width="100" |Resist |
! width="100" |Resist |
||
| Line 17: | Line 31: | ||
! width="75" |Thickness |
! width="75" |Thickness |
||
!Laser (nm) |
!Laser (nm) |
||
! width="125" |Exposure |
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>) |
||
! width="100" |DeFocus |
! width="100" |DeFocus |
||
!Rehydrate* |
|||
! width="75" |PEB |
|||
! width="75" |PEB** |
|||
! width="100" |Developer |
! width="100" |Developer |
||
! width="125" |Developer Time |
! width="125" |Developer Time |
||
! width="300" |Comments |
! width="300" |Comments |
||
|- |
|- |
||
|[[ |
|[[Media:AXP4000pb-Datasheet.pdf|AZ4110]] |
||
|4 krpm |
|4 krpm, 30s |
||
|95°C |
|95°C, 60s |
||
|~ 1.1 µm |
|~ 1.1 µm |
||
|405 |
|405 |
||
| |
|240 |
||
|5 |
|||
| |
| |
||
|''none'' |
|''none'' |
||
|AZ400K:DI 1:4 |
|AZ400K:DI 1:4 |
||
|50s |
|50s |
||
|Used HIMT design (good for isolated lines 0.8-1um) |
|||
| |
|||
|- |
|- |
||
|[[:File:AXP4000pb-Datasheet.pdf|AZ4330]] |
|||
|[[Media:AXP4000pb-Datasheet.pdf|AZ4330]] |
|||
|4 krpm/30s |
|||
|4 krpm, 30s |
|||
|95°C/60s |
|||
|95°C, 60s |
|||
|~ 3.3 µm |
|~ 3.3 µm |
||
|405 |
|405 |
||
| |
|320 |
||
|6 |
|||
| |
| |
||
|''none'' |
|''none'' |
||
|AZ400K:DI 1:4 |
|AZ400K:DI 1:4 |
||
|90s |
|90s |
||
|Used HIMT design |
|||
| |
|||
|- |
|- |
||
|[[: |
|[[Media:AXP4000pb-Datasheet.pdf|AZ4620]] |
||
| |
|||
| |
| |
||
| |
| |
||
| Line 60: | Line 79: | ||
| |
| |
||
|- |
|- |
||
|[[: |
|[[Media:SPR955-Positive-Resist-Datasheet.pdf|SPR 955-CM0.9]] |
||
| |
|3 krpm, 30s |
||
| |
|95°C, 60s |
||
|~ |
|~ 0.9 µm |
||
|405 |
|405 |
||
|250 |
|||
| - 7 |
|||
| |
| |
||
|110°C, 60s |
|||
| |
|||
|115°C/90s |
|||
|AZ300MIF |
|AZ300MIF |
||
|60s |
|60s |
||
|Used by UCSB Staff for tool calibrations/process control. |
|||
|- |
|||
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR 955-1.8]] |
|||
|4 krpm, 30s |
|||
|95°C, 60s |
|||
|~ 1.8 µm |
|||
|405 |
|||
|210 |
|||
|10 |
|||
| |
| |
||
|110°C, 60s |
|||
|AZ300MIF |
|||
|60s |
|||
|Used UCSB design (1um dense lines) |
|||
|- |
|- |
||
|[[: |
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR 220-3.0]] |
||
| |
|2.5 krpm, 30s |
||
| |
|115°C, 90s |
||
|~ |
|~ 2.7 µm |
||
|405 |
|405 |
||
|325 |
|||
| - 4 |
|||
| |
| |
||
|115°C, 90s |
|||
| |
|||
|110°C/60s |
|||
|AZ300MIF |
|AZ300MIF |
||
|60s |
|60s |
||
|Used HIMT design. 0.6-0.9µm line/space. |
|||
| align="left" | |
|||
|- |
|- |
||
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR 220-7.0]] |
|||
|[[:File:3600 D, D2v Spin Speed Curve.pdf|THMR-3600HP]] |
|||
|3.5 krpm, 30s |
|||
| |
|||
|105°C/2min |
|||
| |
|||
Cool 1min |
|||
| |
|||
|~ 7.0µm |
|||
| |
|||
| |
|375 |
||
|~550mJ |
|||
| |
|||
| -20 |
|||
| |
|||
|>1hr |
|||
| |
|||
|115°C, 90s |
|||
| |
|||
|AZ300MiF |
|||
|70s |
|||
|Rehydration after exposure is necessary, to prevent bubbles at PEB. |
|||
|- |
|||
|[[Media:3600 D, D2v Spin Speed Curve.pdf|THMR-3600HP]] |
|||
|1.5 krpm, 45s; |
|||
250 rpm/s |
|||
|100°C, 60s |
|||
|0.430µm |
|||
|405 |
|||
|180–220 |
|||
|<nowiki>-4</nowiki> |
|||
| |
| |
||
|100°C, 60s |
|||
|AZ300MiF |
|||
|20s |
|||
|~0.4nm line/space: |
|||
lower dose for clear-field, higher dose for dark-field. |
|||
|- |
|||
| colspan="12" |*''Rehydration'': After exposure, leave sample in lab air (ok to cover in tray, with tinfoil). Allows water vapor in air to diffuse into PR to complete chemical reaction. |
|||
<nowiki>**</nowiki>''PEB: Post-exposure bake'': after exposure, before develop |
|||
|} |
|} |
||
=== Negative Resist (MLA150) === |
|||
''General notes: Hotplates used, filters, laser wavelengths, etc.'' |
|||
===Negative Resist (MLA150)=== |
|||
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
''We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.'' |
|||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
|||
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
! width="100" |Resist |
! width="100" |Resist |
||
| Line 106: | Line 162: | ||
! width="75" |Thickness |
! width="75" |Thickness |
||
!Laser (nm) |
!Laser (nm) |
||
! width="125" |Exposure |
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>) |
||
! width="100" |DeFocus |
! width="100" |DeFocus |
||
! width="75" |PEB |
! width="75" |PEB* |
||
! width="75" |Flood |
! width="75" |Flood** |
||
! width="100" |Developer |
! width="100" |Developer |
||
! width="125" |Developer Time |
! width="125" |Developer Time |
||
! width="300" |Comments |
! width="300" |Comments |
||
|- |
|- |
||
|[[ |
|[[Media:AZ5214-Negative-Resist-Datasheet.pdf|AZ5214]]** |
||
|6 krpm |
|6 krpm, 30s |
||
|95°C |
|95°C, 60s |
||
|~ 1.0 µm |
|~ 1.0 µm |
||
| |
|375 |
||
| |
|35 |
||
| - 5 |
|||
| |
|||
|110°C, 60s |
|||
| |
|||
|60" |
|60" |
||
|AZ300MIF |
|AZ300MIF |
||
|60s |
|60s |
||
|Used UCSB design. Good for up to ~1.3um open line space. |
|||
| align="left" | |
|||
*??? |
|||
|- |
|- |
||
|[[Media:AZnLOF2020-Negative-Resist-Datasheet.pdf|AZnLOF2020]] |
|||
|AZnLOF2020 |
|||
| |
|4 krpm, 30s |
||
|110°C |
|110°C, 60s |
||
|~ 2.1µm |
|~ 2.1µm |
||
| |
|375 |
||
| |
|340 |
||
| - 3 |
|||
| |
|||
|110°C, 60s |
|||
| |
|||
|''none'' |
|''none'' |
||
|AZ300MIF |
|AZ300MIF |
||
| |
|90s |
||
|Used UCSB design. Good for 2um open line space. |
|||
| |
|||
|- |
|- |
||
|[[ |
|[[Media:SU-8-2075-revA.pdf|SU-8 2075]] |
||
| |
| |
||
| |
| |
||
| Line 153: | Line 208: | ||
| |
| |
||
|Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end. |
|Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end. |
||
|- |
|||
| colspan="12" |*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal |
|||
<nowiki>**</nowiki> To use AZ5214 as a negative PR requires Flood Exposure with the [[Contact Aligner (SUSS MA-6)|MA6]] or [[Suss Aligners (SUSS MJB-3)|MJB]] aligner '''''after PEB''''', before developing. See here for a [[AZ5214 - Basic Process|basic AZ5214 process]], it is different than typical negative resists. |
|||
|} |
|} |
||
=== |
===Greyscale Lithography (MLA150)=== |
||
''AZ4620 is the manufacturer-recommended PR for greyscale litho.'' |
|||
''Description...'' |
|||
{| class="wikitable" border="1" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" |
|||
Please see the [[MLA150 - Design Guidelines#Limitations%20.26%20Workarounds|'''MLA150 - Greyscale Design Guidelines & Limitation''']] |
|||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
|||
|- bgcolor="#D0E7FF" |
|- bgcolor="#D0E7FF" |
||
! width="100" |Resist |
! width="100" |Resist |
||
| Line 163: | Line 223: | ||
! width="75" |Bake |
! width="75" |Bake |
||
! width="75" |Thickness |
! width="75" |Thickness |
||
!Laser |
|||
! width="125" |Exposure Time |
|||
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>) |
|||
! width="100" |Focus Offset |
! width="100" |Focus Offset |
||
!Rehydrate* |
|||
! width="75" |PEB |
|||
! width="75" | |
! width="75" |PEB** |
||
! width="100" |Developer |
! width="100" |Developer |
||
! width="125" |Developer Time |
! width="125" |Developer Time |
||
!Reflow*** |
|||
! width="300" |Comments |
! width="300" |Comments |
||
|- |
|- |
||
|[[Media:Az p4620 photoresist data package.pdf|AZ4620]] |
|||
|AZ4620Z5214 |
|||
| |
|? krpm/30” |
||
|95°C |
|95°C, 60” |
||
| |
|||
|?? µm |
|||
| |
|||
| |
|||
| |
| |
||
| |
| |
||
| |
| |
||
|60" |
|||
|AZ300MIF |
|AZ300MIF |
||
|60s |
|||
| |
|||
| align="left" |''To Be Added'' |
|||
|- |
|||
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR 220-7.0]] |
|||
|3.5 krpm, 30s |
|||
|105°C/2min |
|||
Cool 1min |
|||
|~ 7.0µm |
|||
|375 |
|||
|~624mJ to clear large mm-area, |
|||
520mJ to clear ~5µm lines. |
|||
| -20 |
|||
|≥1hr |
|||
|115°C, 90s |
|||
|AZ300MiF |
|||
|70s |
|||
|TBD |
|||
|<small>Author Credit:</small> |
|||
*<small>Patrick Curtis, 2022</small> |
|||
*<small>Biljana Stamenic 2023</small> |
|||
*<small>Demis D. John 2023</small> |
|||
|- |
|||
| |
|||
| colspan="12" |Notes on SPR 220-7 Greyscale: Rehydration after exposure is necessary, to prevent bubbles at PEB. |
|||
Stitching leaves ridges in Y-direction with ~5% height of removed PR depth. Can be reduced via reflow, but significantly affects PR profile. |
|||
<small>Author Credit: Patrick Curtis, 2022 & Biljana Stamenic 2023 & Demis D. John 2023; Please see our [[Frequently Asked Questions#Publications acknowledging the Nanofab|publications policy]].</small> |
|||
|- |
|||
| colspan="13" |*''Rehydration'': After exposure, leave sample in lab air (ok to cover in tray, with tinfoil). Allows water vapor in air to diffuse into PR to complete chemical reaction. |
|||
<nowiki>**</nowiki>''PEB: Post-exposure bake'': after exposure, before develop |
|||
<nowiki>***</nowiki>''Reflow'': To smooth out stitching lines. Will change sharp vertical profiles considerably, only good for gradually-sloped profiles. |
|||
|} |
|||
== [[E-Beam Lithography System (Raith EBPG 5150+)|E-Beam Lithography Recipes (Raith EBPG 5150+)]] == |
|||
=== Electron Beam Resists Available === |
|||
EBL Resists are custom-mixed according to user resolution needs - contact [[Bill Mitchell]] to get a bottle. |
|||
Currently available at UCSB are: |
|||
*'''PMMA''': (950K in anisole, 950K in MIBK, 495K in anisole, 50K in anisole) |
|||
**High-resolution positive polymer-based resist with relatively poor sensitivity (resolution scales directly and sensitivity scales inversely with molecular weight); |
|||
**Poor plasma etch resistance, hence used primarily to fabricate metal lines via liftoff processes (via a bi-layer resist scheme...low MW on bottom, high MW on top for single lines, or vice-versa for T-gate fabrication); |
|||
**Utilizes an inert solvent developer (usually MIBK:IPA mixtures) |
|||
*'''P(MMA-MAA) copolymer''': (low MW methyl-methacrylate (MMA) and methacrylic acid (MAA) copolymers in ethyl lactate) |
|||
**A positive polymer-based resist with poor resolution but with significantly higher sensitivity than the higher MW PMMA resists above |
|||
**Used primarily as the top layer in a bi-layer resist scheme for T-Gate fabrication, and utilizes inert solvent developer (MIBK:IPA mixtures) |
|||
*'''CSAR-62''': ZEP-equivalent resist manufactured in Germany at much more competitive pricing! |
|||
**High-resolution polymer-based positive resist with very good sensitivity and excellent etch resistance |
|||
**Can be used in both metal lift-off processes (slight overexposure results in an excellent undercut profile) and various dry-etch processes for pattern transfer to the underlying substrate |
|||
**Utilizes inert solvent developers (e.g., n-amyl acetate for higher sensitivity and good resolution or MIBK:IPA mixtures for increased LER performance) |
|||
*'''maN-2403''': negative polymer-based resist (that is NOT chemically amplified) |
|||
**Very good resolution (down to the 40-50nm range) and sensitivity |
|||
**Exhibits excellent dry-etch resistance |
|||
**Developed using a dilute basic solution (e.g., metal-ion-free developers such as AZ-300MIF) |
|||
*'''HSQ''': negative resist that is based on spin-on glass material (ie, not polymer-based) |
|||
**Extremely good resolution (features below 10nm can be resolved) |
|||
**Etch resistance is high in Cl-based chemistries since HSQ reduces to a porous SiOx structure after exposure and development |
|||
**Sensitivity and contrast are very dependent on developer solution used and are usually poor |
|||
***Standard AZ300MIF developer solutions have decent sensitivity (100's of uC/cm2 at 100kV) but extremely poor contrast |
|||
***Stronger (and toxic!) 25%TMAH solutions have much better contrast but poor sensitivity (1000's of uC/cm2 at 100kV) |
|||
***"Salty" developer solutions using 1wt% NaCl dissolved in either 4wt% NaOH or AZ300MIF solutions have the best contrast but reduce sensitivity significantly (10,000's of uC/cm2 at 100kV) |
|||
*'''DUV resists: UV6, UV210 UVN-30''': chemically amplified polymer-based resists |
|||
**High resolution and excellent sensitivity (clearing doses below 100uC/cm2 at 100kV) |
|||
**UV6 used mostly in optimized t-gate resist structures |
|||
**Developed using a dilute basic solution (e.g., metal-ion-free developers such as AZ-300MIF) |
|||
**Can be "double exposed" by [[Stepper 3 (ASML DUV)|ASML DUV Stepper]] and EBL. |
|||
***Recommended to produce ASML alignment marks first for double exposure methods. |
|||
**See ASML litho recipes for datasheets. |
|||
=== EBL Exposure Recipes === |
|||
'''''To Be Added''''' - BEAMER simulation is always required for small (<<micron) features. |
|||
=== Alignment Marks === |
|||
* 20µm square is the std. [[E-Beam Lithography System (Raith EBPG 5150+)|Raith EBL]] Alignment Marker. Place in known coordinate of every die.<br /> |
|||
==[[Maskless Aligner (Raith PicoMaster XF)|Maskless Aligner (Raith PicoMasterXF)]] == |
|||
=== Positive Resist (Raith PicoMasterXF) === |
|||
=== <small>Note: Calibrations done with the "UCSB design" on 4 inch Si wafers, using resists listed below. Used exposure recipe " 200um_GLV".</small> === |
|||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
|||
|- bgcolor="#D0E7FF" |
|||
! width="100" |Resist |
|||
! width="100" |Spin Cond. |
|||
! width="75" |Bake |
|||
! width="75" |Thickness |
|||
!Laser (nm) |
|||
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>) |
|||
! width="100" |DeFocus |
|||
!Rehydrate* |
|||
! width="75" |PEB** |
|||
! width="100" |Developer |
|||
! width="125" |Developer Time |
|||
! width="300" |Comments |
|||
|- |
|||
|[[Media:AXP4000pb-Datasheet.pdf|AZ4110]] |
|||
|4 krpm, 30s |
|||
|95°C, 60s |
|||
|~ 1.1 µm |
|||
|405 |
|||
|130 |
|||
|0 |
|||
| |
|||
|''none'' |
|||
|AZ400K:DI 1:4 |
|||
|50s |
|||
|Used UCSB design |
|||
(dense line/gap, 0.65um/0.65um) |
|||
|- |
|||
|[[Media:AXP4000pb-Datasheet.pdf|AZ4330]] |
|||
|4 krpm, 30s |
|||
|95°C, 60s |
|||
|~ 3.3 µm |
|||
|405 |
|||
|200 |
|||
| -1 |
|||
| |
|||
|''none'' |
|||
|AZ400K:DI 1:4 |
|||
|90s |
|||
|Used UCSB design |
|||
(dense line/gap, 1um/1um) |
|||
|- |
|||
|[[Media:SPR955-Positive-Resist-Datasheet.pdf|SPR 955-CM0.9]] |
|||
|3 krpm, 30s |
|||
|95°C, 60s |
|||
|~ 0.9 µm |
|||
|405 |
|||
|100 |
|||
| -1.5 |
|||
| |
|||
|110°C, 60s |
|||
|AZ300MIF |
|||
|60s |
|||
|Used UCSB design |
|||
(dense line/gap, 0.6um/0.6um) |
|||
Vertical lines~602nm, Horizontal lines~454nm |
|||
|- |
|||
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR 955-1.8]] |
|||
|4 krpm, 30s |
|||
|95°C, 60s |
|||
|~ 1.8 µm |
|||
|405 |
|||
|200 |
|||
|0 |
|||
| |
|||
|110°C, 60s |
|||
|AZ300MIF |
|||
|60s |
|||
|Used UCSB design |
|||
(dense line/gap, 0.6um/0.6um) |
|||
|- |
|||
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR 220-3.0]] |
|||
|2.5 krpm, 30s |
|||
|115°C, 90s |
|||
|~ 2.7 µm |
|||
|405 |
|||
|180 |
|||
| -1 |
|||
| |
|||
|115°C, 90s |
|||
|AZ300MIF |
|||
|60s |
|||
|Used UCSB design |
|||
(dense line/gap, 0.65um/0.65um) |
|||
|- |
|||
|[[Media:SPR220-Positive-Resist-Datasheet.pdf|SPR 220-7.0]] |
|||
|3.5 krpm, 30s |
|||
|105°C/2min |
|||
Cool 1min |
|||
|~ 7.0µm |
|||
|405 |
|||
|340 |
|||
| -3 |
|||
|>1hr |
|||
|115°C, 90s |
|||
|AZ300MiF |
|||
|70s |
|||
|Used UCSB design |
|||
(dense line/gap, >>1um/1um) |
|||
|} |
|||
===Negative Resist (Raith PicoMasterXF)=== |
|||
Note: Calibrations done with the "UCSB design" on 4 inch Si wafers, using resists listed below. |
|||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
|||
|- bgcolor="#D0E7FF" |
|||
! width="100" |Resist |
|||
! width="100" |Spin Cond. |
|||
! width="75" |Bake |
|||
! width="75" |Thickness |
|||
!Laser (nm) |
|||
! width="125" |Exposure Dose (mJ/cm<sup>2</sup>) |
|||
! width="100" |DeFocus |
|||
! width="75" |PEB* |
|||
! width="75" |Flood** |
|||
! width="100" |Developer |
|||
! width="125" |Developer Time |
|||
! width="300" |Comments |
|||
|- |
|||
|[[Media:AZ5214-Negative-Resist-Datasheet.pdf|AZ5214]]** |
|||
|6 krpm, 30s |
|||
|95°C, 60s |
|||
|~ 1.0 µm |
|||
|405 |
|||
|30 |
|||
|0 |
|||
|110°C, 60s |
|||
|60" |
|60" |
||
|AZ300MIF |
|||
| align="left" | |
|||
|60s |
|||
*??? |
|||
|Used UCSB design (dense lines are patterned negative resist) (line/gap=1um/1um) |
|||
|- |
|||
|[[Media:AZnLOF2020-Negative-Resist-Datasheet.pdf|AZnLOF2020]] |
|||
|4 krpm, 30s |
|||
|110°C, 60s |
|||
|~ 2.1µm |
|||
|405 |
|||
|450 (or higher) |
|||
| +2 |
|||
|110°C, 60s |
|||
|''none'' |
|||
|AZ300MIF |
|||
|30s |
|||
|Used UCSB design (dense lines are patterned negative resist) (line/gap=1um/1um) |
|||
|- |
|||
|} |
|} |
||
<nowiki>*</nowiki>PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal |
|||
<nowiki>**</nowiki> To use AZ5214 as a negative PR requires Flood Exposure with the [[Contact Aligner (SUSS MA-6)|MA6]] or [[Suss Aligners (SUSS MJB-3)|MJB]] aligner '''''after PEB''''', before developing. See here for a [[AZ5214 - Basic Process|basic AZ5214 process]], it is different than typical negative resists. |
|||
Latest revision as of 01:49, 14 November 2026
Maskless Aligner (Heidelberg MLA150)
For CAD design tips and requirements, see these pages:
- Design Guidelines + Tips - useful info for designing your CAD files, alignment marks etc.
- CAD Files and Templates - example CAD files etc.
Photolithography Recipes for the Heidelberg MLA150. All recipes were characterized on blank Silicon wafers. For different substrate coatings/materials, you will likely need to run a focus-exposure matrix ("series" exposure mode), using our params as a starting point.
These recipes use the same spin and bake params as our contact aligner and stepper recipes, using built-in hotplates on the photoresist spinner benches.
Any I-Line PR is usable, although we only characterized a select few below. Run your own Focus-Exposure Matrix to characterize a new PR.
Note: On this tool, it is common to have to run a Focus-Exposure Matrix (aka. FEM), via "Series" exposure mode, for each new layer structure and/or critical feature size. The layer structure can strongly affect the exposure parameters. See the FEM Analysis Tips page for how to choose the proper exposure parameters.
The MLA Troubleshooting > Out-of-Focus Exposures section can help you avoid bad exposures, please read it!
Positive Resist (MLA150)
We found that positive PR's worked well with the 405nm laser - the 375nm laser would likely also work. Sub-micron features are possible. Overexposure is recommended to avoid stitching and horiz/vert discrepancies; compensate for widening/narrowing using CD Bias as described here.
Note: calibrations done with the "HIMT design" will show higher dose, due to using only dark-field line/space patterns.
| Resist | Spin Cond. | Bake | Thickness | Laser (nm) | Exposure Dose (mJ/cm2) | DeFocus | Rehydrate* | PEB** | Developer | Developer Time | Comments |
|---|---|---|---|---|---|---|---|---|---|---|---|
| AZ4110 | 4 krpm, 30s | 95°C, 60s | ~ 1.1 µm | 405 | 240 | 5 | none | AZ400K:DI 1:4 | 50s | Used HIMT design (good for isolated lines 0.8-1um) | |
| AZ4330 | 4 krpm, 30s | 95°C, 60s | ~ 3.3 µm | 405 | 320 | 6 | none | AZ400K:DI 1:4 | 90s | Used HIMT design | |
| AZ4620 | |||||||||||
| SPR 955-CM0.9 | 3 krpm, 30s | 95°C, 60s | ~ 0.9 µm | 405 | 250 | - 7 | 110°C, 60s | AZ300MIF | 60s | Used by UCSB Staff for tool calibrations/process control. | |
| SPR 955-1.8 | 4 krpm, 30s | 95°C, 60s | ~ 1.8 µm | 405 | 210 | 10 | 110°C, 60s | AZ300MIF | 60s | Used UCSB design (1um dense lines) | |
| SPR 220-3.0 | 2.5 krpm, 30s | 115°C, 90s | ~ 2.7 µm | 405 | 325 | - 4 | 115°C, 90s | AZ300MIF | 60s | Used HIMT design. 0.6-0.9µm line/space. | |
| SPR 220-7.0 | 3.5 krpm, 30s | 105°C/2min
Cool 1min |
~ 7.0µm | 375 | ~550mJ | -20 | >1hr | 115°C, 90s | AZ300MiF | 70s | Rehydration after exposure is necessary, to prevent bubbles at PEB. |
| THMR-3600HP | 1.5 krpm, 45s;
250 rpm/s |
100°C, 60s | 0.430µm | 405 | 180–220 | -4 | 100°C, 60s | AZ300MiF | 20s | ~0.4nm line/space:
lower dose for clear-field, higher dose for dark-field. | |
| *Rehydration: After exposure, leave sample in lab air (ok to cover in tray, with tinfoil). Allows water vapor in air to diffuse into PR to complete chemical reaction.
**PEB: Post-exposure bake: after exposure, before develop | |||||||||||
Negative Resist (MLA150)
We found that all the negative PR's we tested required the 375nm in order to be fully exposed with reasonable dose/time.
| Resist | Spin Cond. | Bake | Thickness | Laser (nm) | Exposure Dose (mJ/cm2) | DeFocus | PEB* | Flood** | Developer | Developer Time | Comments |
|---|---|---|---|---|---|---|---|---|---|---|---|
| AZ5214** | 6 krpm, 30s | 95°C, 60s | ~ 1.0 µm | 375 | 35 | - 5 | 110°C, 60s | 60" | AZ300MIF | 60s | Used UCSB design. Good for up to ~1.3um open line space. |
| AZnLOF2020 | 4 krpm, 30s | 110°C, 60s | ~ 2.1µm | 375 | 340 | - 3 | 110°C, 60s | none | AZ300MIF | 90s | Used UCSB design. Good for 2um open line space. |
| SU-8 2075 | ~70µm | 375 | Extremely viscous. Pour into a wide-mouthed bottle, dispense directly from bottle. Replace napkin at end. | ||||||||
| *PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal
** To use AZ5214 as a negative PR requires Flood Exposure with the MA6 or MJB aligner after PEB, before developing. See here for a basic AZ5214 process, it is different than typical negative resists. | |||||||||||
Greyscale Lithography (MLA150)
AZ4620 is the manufacturer-recommended PR for greyscale litho.
Please see the MLA150 - Greyscale Design Guidelines & Limitation
| Resist | Spin Cond. | Bake | Thickness | Laser | Exposure Dose (mJ/cm2) | Focus Offset | Rehydrate* | PEB** | Developer | Developer Time | Reflow*** | Comments |
|---|---|---|---|---|---|---|---|---|---|---|---|---|
| AZ4620 | ? krpm/30” | 95°C, 60” | AZ300MIF | 60s | To Be Added | |||||||
| SPR 220-7.0 | 3.5 krpm, 30s | 105°C/2min
Cool 1min |
~ 7.0µm | 375 | ~624mJ to clear large mm-area,
520mJ to clear ~5µm lines. |
-20 | ≥1hr | 115°C, 90s | AZ300MiF | 70s | TBD | Author Credit:
|
| Notes on SPR 220-7 Greyscale: Rehydration after exposure is necessary, to prevent bubbles at PEB.
Stitching leaves ridges in Y-direction with ~5% height of removed PR depth. Can be reduced via reflow, but significantly affects PR profile. Author Credit: Patrick Curtis, 2022 & Biljana Stamenic 2023 & Demis D. John 2023; Please see our publications policy. | ||||||||||||
| *Rehydration: After exposure, leave sample in lab air (ok to cover in tray, with tinfoil). Allows water vapor in air to diffuse into PR to complete chemical reaction.
**PEB: Post-exposure bake: after exposure, before develop ***Reflow: To smooth out stitching lines. Will change sharp vertical profiles considerably, only good for gradually-sloped profiles. | ||||||||||||
E-Beam Lithography Recipes (Raith EBPG 5150+)
Electron Beam Resists Available
EBL Resists are custom-mixed according to user resolution needs - contact Bill Mitchell to get a bottle.
Currently available at UCSB are:
- PMMA: (950K in anisole, 950K in MIBK, 495K in anisole, 50K in anisole)
- High-resolution positive polymer-based resist with relatively poor sensitivity (resolution scales directly and sensitivity scales inversely with molecular weight);
- Poor plasma etch resistance, hence used primarily to fabricate metal lines via liftoff processes (via a bi-layer resist scheme...low MW on bottom, high MW on top for single lines, or vice-versa for T-gate fabrication);
- Utilizes an inert solvent developer (usually MIBK:IPA mixtures)
- P(MMA-MAA) copolymer: (low MW methyl-methacrylate (MMA) and methacrylic acid (MAA) copolymers in ethyl lactate)
- A positive polymer-based resist with poor resolution but with significantly higher sensitivity than the higher MW PMMA resists above
- Used primarily as the top layer in a bi-layer resist scheme for T-Gate fabrication, and utilizes inert solvent developer (MIBK:IPA mixtures)
- CSAR-62: ZEP-equivalent resist manufactured in Germany at much more competitive pricing!
- High-resolution polymer-based positive resist with very good sensitivity and excellent etch resistance
- Can be used in both metal lift-off processes (slight overexposure results in an excellent undercut profile) and various dry-etch processes for pattern transfer to the underlying substrate
- Utilizes inert solvent developers (e.g., n-amyl acetate for higher sensitivity and good resolution or MIBK:IPA mixtures for increased LER performance)
- maN-2403: negative polymer-based resist (that is NOT chemically amplified)
- Very good resolution (down to the 40-50nm range) and sensitivity
- Exhibits excellent dry-etch resistance
- Developed using a dilute basic solution (e.g., metal-ion-free developers such as AZ-300MIF)
- HSQ: negative resist that is based on spin-on glass material (ie, not polymer-based)
- Extremely good resolution (features below 10nm can be resolved)
- Etch resistance is high in Cl-based chemistries since HSQ reduces to a porous SiOx structure after exposure and development
- Sensitivity and contrast are very dependent on developer solution used and are usually poor
- Standard AZ300MIF developer solutions have decent sensitivity (100's of uC/cm2 at 100kV) but extremely poor contrast
- Stronger (and toxic!) 25%TMAH solutions have much better contrast but poor sensitivity (1000's of uC/cm2 at 100kV)
- "Salty" developer solutions using 1wt% NaCl dissolved in either 4wt% NaOH or AZ300MIF solutions have the best contrast but reduce sensitivity significantly (10,000's of uC/cm2 at 100kV)
- DUV resists: UV6, UV210 UVN-30: chemically amplified polymer-based resists
- High resolution and excellent sensitivity (clearing doses below 100uC/cm2 at 100kV)
- UV6 used mostly in optimized t-gate resist structures
- Developed using a dilute basic solution (e.g., metal-ion-free developers such as AZ-300MIF)
- Can be "double exposed" by ASML DUV Stepper and EBL.
- Recommended to produce ASML alignment marks first for double exposure methods.
- See ASML litho recipes for datasheets.
EBL Exposure Recipes
To Be Added - BEAMER simulation is always required for small (<<micron) features.
Alignment Marks
- 20µm square is the std. Raith EBL Alignment Marker. Place in known coordinate of every die.
Maskless Aligner (Raith PicoMasterXF)
Positive Resist (Raith PicoMasterXF)
Note: Calibrations done with the "UCSB design" on 4 inch Si wafers, using resists listed below. Used exposure recipe " 200um_GLV".
| Resist | Spin Cond. | Bake | Thickness | Laser (nm) | Exposure Dose (mJ/cm2) | DeFocus | Rehydrate* | PEB** | Developer | Developer Time | Comments |
|---|---|---|---|---|---|---|---|---|---|---|---|
| AZ4110 | 4 krpm, 30s | 95°C, 60s | ~ 1.1 µm | 405 | 130 | 0 | none | AZ400K:DI 1:4 | 50s | Used UCSB design
(dense line/gap, 0.65um/0.65um) | |
| AZ4330 | 4 krpm, 30s | 95°C, 60s | ~ 3.3 µm | 405 | 200 | -1 | none | AZ400K:DI 1:4 | 90s | Used UCSB design
(dense line/gap, 1um/1um) | |
| SPR 955-CM0.9 | 3 krpm, 30s | 95°C, 60s | ~ 0.9 µm | 405 | 100 | -1.5 | 110°C, 60s | AZ300MIF | 60s | Used UCSB design
(dense line/gap, 0.6um/0.6um) Vertical lines~602nm, Horizontal lines~454nm | |
| SPR 955-1.8 | 4 krpm, 30s | 95°C, 60s | ~ 1.8 µm | 405 | 200 | 0 | 110°C, 60s | AZ300MIF | 60s | Used UCSB design
(dense line/gap, 0.6um/0.6um) | |
| SPR 220-3.0 | 2.5 krpm, 30s | 115°C, 90s | ~ 2.7 µm | 405 | 180 | -1 | 115°C, 90s | AZ300MIF | 60s | Used UCSB design
(dense line/gap, 0.65um/0.65um) | |
| SPR 220-7.0 | 3.5 krpm, 30s | 105°C/2min
Cool 1min |
~ 7.0µm | 405 | 340 | -3 | >1hr | 115°C, 90s | AZ300MiF | 70s | Used UCSB design
(dense line/gap, >>1um/1um) |
Negative Resist (Raith PicoMasterXF)
Note: Calibrations done with the "UCSB design" on 4 inch Si wafers, using resists listed below.
| Resist | Spin Cond. | Bake | Thickness | Laser (nm) | Exposure Dose (mJ/cm2) | DeFocus | PEB* | Flood** | Developer | Developer Time | Comments |
|---|---|---|---|---|---|---|---|---|---|---|---|
| AZ5214** | 6 krpm, 30s | 95°C, 60s | ~ 1.0 µm | 405 | 30 | 0 | 110°C, 60s | 60" | AZ300MIF | 60s | Used UCSB design (dense lines are patterned negative resist) (line/gap=1um/1um) |
| AZnLOF2020 | 4 krpm, 30s | 110°C, 60s | ~ 2.1µm | 405 | 450 (or higher) | +2 | 110°C, 60s | none | AZ300MIF | 30s | Used UCSB design (dense lines are patterned negative resist) (line/gap=1um/1um) |
*PEB: post-exposure bake. For AZ 5214-IR, this performs Image Reversal
** To use AZ5214 as a negative PR requires Flood Exposure with the MA6 or MJB aligner after PEB, before developing. See here for a basic AZ5214 process, it is different than typical negative resists.