Lithography Recipes: Difference between revisions
→Lift-Off Recipes: corrected LOR30C to 2-3µm |
|||
| (45 intermediate revisions by 5 users not shown) | |||
| Line 21: | Line 21: | ||
#***[[Stepper Recipes#Stepper 3 .28ASML DUV.29|Stepper #3: ASML PAS 5500/300]] (DUV) |
#***[[Stepper Recipes#Stepper 3 .28ASML DUV.29|Stepper #3: ASML PAS 5500/300]] (DUV) |
||
#**[[Direct-Write Lithography Recipes|<u>Direct-Write Recipes</u>]] |
#**[[Direct-Write Lithography Recipes|<u>Direct-Write Recipes</u>]] |
||
#***[[Direct-Write Lithography Recipes#Maskless Aligner .28Heidelberg MLA150.29|Heidelberg MLA150]] |
#***[[Direct-Write Lithography Recipes#Maskless Aligner .28Heidelberg MLA150.29|Heidelberg MLA150 (I-Line)]] |
||
#***[[Lithography Recipes#E-Beam Lithography Recipes| |
#***[[Direct-Write Lithography Recipes#E-Beam Lithography Recipes (Raith EBPG 5150+)|Raith EBPG 5150+ (Electron-Beam)]] |
||
#***[[Lithography Recipes#FIB Lithography Recipes .28Raith Velion.29|Raith Velion FIB]] |
#***[[Lithography Recipes#FIB Lithography Recipes .28Raith Velion.29|Raith Velion FIB (Ion Beam)]] |
||
#**[[Lithography Recipes#Automated Coat.2FDevelop System Recipes .28S-Cubed Flexi.29|Automated Coater Recipes (S-Cubed Flexi)]] |
#**[[Lithography Recipes#Automated Coat.2FDevelop System Recipes .28S-Cubed Flexi.29|Automated Coater Recipes (S-Cubed Flexi)]] |
||
#[[Lithography Recipes#General Photolithography Techniques|'''General Photolithography Techniques''']] |
#[[Lithography Recipes#General Photolithography Techniques|'''General Photolithography Techniques''']] |
||
#*''Techniques for improving litho. or solving common photolith. problems.'' |
#*''Techniques for improving litho. or solving common photolith. problems.'' |
||
#*[[Photolithography - Improving Adhesion Photoresist Adhesion|HMDS Process for Improving Adhesion]] |
|||
#*[[Photolithography - Manual Edge-Bead Removal Techniques|Edge-Bead Removal Techniques]] |
|||
#*[https://www.microchemicals.com/technical_information/reflow_photoresist.pdf Photoresist reflow (MicroChem)] |
|||
#*[[Lithography Calibration - Analyzing a Focus-Exposure Matrix]] |
|||
#'''[[Lithography Recipes#Lift-Off Recipes|Lift-Off Recipes]]''' |
#'''[[Lithography Recipes#Lift-Off Recipes|Lift-Off Recipes]]''' |
||
#*''Verified Recipes for lift-off using various photolith. tools'' |
#*''Verified Recipes for lift-off using various photolith. tools'' |
||
| Line 81: | Line 85: | ||
*''These techniques are required for loading full-wafers into etchers that use top-side clamps, to prevent photoresist from sticking to the clamp (and potentially destroying your wafer).'' |
*''These techniques are required for loading full-wafers into etchers that use top-side clamps, to prevent photoresist from sticking to the clamp (and potentially destroying your wafer).'' |
||
*''For contact lithography, this improves the proximity of the mask plate and sample, improving resolution. For some projection systems, such as the [[Maskless Aligner (Heidelberg MLA150)|Maskless Aligner]], EBR can help with autofocus issues.'' |
*''For contact lithography, this improves the proximity of the mask plate and sample, improving resolution. For some projection systems, such as the [[Maskless Aligner (Heidelberg MLA150)|Maskless Aligner]], EBR can help with autofocus issues.'' |
||
*''For small samples (<1cm) some techniques here to reduce edge-bead via shims.'' |
|||
====[https://www.microchemicals.com/technical_information/reflow_photoresist.pdf '''Photoresist reflow (MicroChem)''']==== |
====[https://www.microchemicals.com/technical_information/reflow_photoresist.pdf '''Photoresist reflow (MicroChem)''']==== |
||
*''To create slanted sidewalls or curved surfaces.'' |
*''To create slanted sidewalls or curved surfaces.'' |
||
[[Lithography Calibration - Analyzing a Focus-Exposure Matrix|'''Lithography Calibration - Analyzing a Focus-Exposure Matrix''']] |
|||
* ''On tools with autofocus (steppers & direct-write litho tools), you calibrate your litho by shooting a "Focus Exposure Matrix/Array", or "FEM/FEA", which exposes a grid with Dose varying in one axis, and Focus varying in the other.'' |
|||
* ''Explains how to locate the'' ''"Process Window" for your lithography.'' |
|||
==Photolithography Recipes== |
==Photolithography Recipes== |
||
==== Process Maturity Ranking ==== |
|||
*<small>'''R''': ''Recipe is available. Clicking this link will take you to the recipe.''</small> |
|||
*<small>'''A''': ''Material is available for use, but no recipes are provided.''</small> |
|||
* <code>'''R6'''</code> - most mature process with regular calibrations recorded on SPC charts. |
|||
* … |
|||
* <code>'''R1'''</code> - least mature - "possible" but you'll have to figure it out. |
|||
* '''<code>A</code>''': Material is available for use, but no recipes are provided. |
|||
''The Key/Legend for this table's <code>R1...R6</code> values is at the <u>[[Lithography Recipes#Process Ranking Table|bottom of the table]]</u>.'' |
|||
''Click the tool title to go to recipes for that tool.'' |
''Click the tool title to go to recipes for that tool.'' |
||
| Line 96: | Line 111: | ||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" |
||
|- |
|- |
||
! colspan=" |
! colspan="8" height="45" |<div style="font-size: 150%;">Photolithography Recipes</div> |
||
|- |
|- |
||
| Line 102: | Line 117: | ||
! colspan="2" align="center" |'''[[Contact Alignment Recipes|<big>Contact Aligner Recipes</big>]]''' |
! colspan="2" align="center" |'''[[Contact Alignment Recipes|<big>Contact Aligner Recipes</big>]]''' |
||
! colspan="3" align="center" |'''[[Stepper Recipes|<big>Stepper Recipes</big>]]''' |
! colspan="3" align="center" |'''[[Stepper Recipes|<big>Stepper Recipes</big>]]''' |
||
! align="center" |[[Direct-Write Lithography Recipes|Direct-Write Litho. Recipes]] |
! colspan="2" align="center" |[[Direct-Write Lithography Recipes|Direct-Write Litho. Recipes]] |
||
|- |
|- |
||
! width="150" bgcolor="#D0E7FF" align="center" |'''Positive Resists''' |
! width="150" bgcolor="#D0E7FF" align="center" |'''Positive Resists''' |
||
{{LithRecipe Table}} |
{{LithRecipe Table}} |
||
|Picomaster XF200 (Raith) |
|||
|- bgcolor="EEFFFF"<!-- This is the Row color: lightblue --> |
|- bgcolor="EEFFFF"<!-- This is the Row color: lightblue --> |
||
| bgcolor="#D0E7FF" align="center" |[[:File:AXP4000pb-Datasheet.pdf|AZ4110]] |
| bgcolor="#D0E7FF" align="center" |[[:File:AXP4000pb-Datasheet.pdf|AZ4110]] |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)|R1}} |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
||
|A |
|A |
||
| Line 114: | Line 130: | ||
| |
| |
||
|{{rl|MLA_Recipes|Positive Resist (MLA 150)}} |
|{{rl|MLA_Recipes|Positive Resist (MLA 150)}} |
||
|{{rl|Direct-Write Lithography Recipes|Positive Resist (Raith PicoMaster)}} |
|||
|-<!-- This is a White row color --> |
|-<!-- This is a White row color --> |
||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/f/fc/AXP4000pb-Datasheet.pdf AZ4210] |
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/f/fc/AXP4000pb-Datasheet.pdf AZ4210] |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)|R1}} |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
||
|A |
|A |
||
| Line 130: | Line 148: | ||
| |
| |
||
|{{rl|MLA_Recipes|Positive Resist (MLA 150)}} |
|{{rl|MLA_Recipes|Positive Resist (MLA 150)}} |
||
|{{rl|Direct-Write Lithography Recipes|Positive Resist (Raith PicoMaster)|R1}} |
|||
|- |
|- |
||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/a/a2/Az_p4620_photoresist_data_package.pdf AZ4620] |
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/a/a2/Az_p4620_photoresist_data_package.pdf AZ4620] |
||
| Line 150: | Line 170: | ||
|A |
|A |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
||
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)}} |
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)|R3}} |
||
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} |
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)|R5}} |
||
| |
| |
||
|{{rl|MLA Recipes|Positive Resist (MLA 150)}} |
|{{rl|MLA Recipes|Positive Resist (MLA 150)|R3}} |
||
|{{rl|Direct-Write Lithography Recipes|Positive Resist (Raith)|R3}} |
|||
|- |
|- |
||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/2/29/SPR955-Positive-Resist-Datasheet.pdf SPR 955 CM-1.8] |
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/2/29/SPR955-Positive-Resist-Datasheet.pdf SPR 955 CM-1.8] |
||
|A |
|A |
||
|A |
|A |
||
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)}} |
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)|R3}} |
||
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} |
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)|R3}} |
||
| |
| |
||
|{{rl|MLA Recipes|Positive Resist (MLA 150)|R3}} |
|||
|A |
|||
|- bgcolor="EEFFFF" |
|- bgcolor="EEFFFF" |
||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/3f/SPR220-Positive-Resist-Datasheet.pdf SPR 220-3.0] |
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/3f/SPR220-Positive-Resist-Datasheet.pdf SPR 220-3.0] |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
||
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)}} |
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)|R3}} |
||
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} |
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)|R3}} |
||
| |
| |
||
|{{rl|MLA Recipes|Positive Resist (MLA 150)}} |
|{{rl|MLA Recipes|Positive Resist (MLA 150)}} |
||
| Line 174: | Line 195: | ||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
||
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)}} |
|{{rl|Stepper Recipes|Positive Resist (GCA 6300)|R3}} |
||
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} |
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)|R3}} |
||
| |
| |
||
|{{rl|MLA Recipes|Positive_Resist_.28MLA150.29}} |
|{{rl|MLA Recipes|Positive_Resist_.28MLA150.29}} |
||
| Line 192: | Line 213: | ||
| |
| |
||
| |
| |
||
|{{rl|Stepper Recipes|Positive Resist (ASML DUV)}} |
|{{rl|Stepper Recipes|Positive Resist (ASML DUV)|R5}} |
||
| |
| |
||
|- bgcolor="EEFFFF" |
|- bgcolor="EEFFFF" |
||
| Line 213: | Line 234: | ||
! bgcolor="#D0E7FF" align="center" |'''Negative Resists''' |
! bgcolor="#D0E7FF" align="center" |'''Negative Resists''' |
||
{{LithRecipe Table}} |
{{LithRecipe Table}} |
||
|Picomaster XF200 (Raith) |
|||
|- |
|- |
||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/b/b0/AZ5214-Negative-Resist-Datasheet.pdf AZ5214-EIR] |
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/b/b0/AZ5214-Negative-Resist-Datasheet.pdf AZ5214-EIR] |
||
| Line 225: | Line 247: | ||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MJB-3)}} |
||
|{{rl|Contact_Alignment_Recipes|Negative Resist (MA-6)}} |
|{{rl|Contact_Alignment_Recipes|Negative Resist (MA-6)}} |
||
|{{rl|Stepper Recipes|Negative Resist (GCA 6300)}} |
|{{rl|Stepper Recipes|Negative Resist (GCA 6300)|R3}} |
||
|{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} |
|{{rl|Stepper Recipes|Negative Resist (AutoStep 200)|R3}} |
||
| |
| |
||
|{{rl|MLA Recipes|Negative Resist (MLA 150)}} |
|{{rl|MLA Recipes|Negative Resist (MLA 150)|R3}} |
||
|- |
|- |
||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/5/5e/AZnLOF2020-Negative-Resist-Datasheet.pdf AZnLOF 2035] |
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/5/5e/AZnLOF2020-Negative-Resist-Datasheet.pdf AZnLOF 2035] |
||
| bgcolor=" |
| bgcolor="#D0E7FF" |A |
||
| {{rl|Contact_Alignment_Recipes|Negative Resist (MA-6)|R1}} |
|||
| bgcolor="EEFFFF" |A |
|||
| bgcolor="EEFFFF" |A |
| bgcolor="EEFFFF" |A |
||
| bgcolor="EEFFFF" |A |
| bgcolor="EEFFFF" |A |
||
| Line 241: | Line 263: | ||
|A |
|A |
||
|A |
|A |
||
|{{Rl|Stepper_Recipes|Negative_Resist_.28GCA_6300.29|R2}} |
|||
|A |
|||
|A |
|A |
||
| |
| |
||
| Line 259: | Line 281: | ||
| |
| |
||
| |
| |
||
|{{rl|Stepper Recipes|Negative Resist (ASML DUV)}} |
|{{rl|Stepper Recipes|Negative Resist (ASML DUV)|R6}} |
||
| |
| |
||
|- |
|- |
||
| Line 282: | Line 304: | ||
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
|{{rl|Contact_Alignment_Recipes|Positive Resist (MA-6)}} |
||
|A |
|A |
||
|{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} |
|{{rl|Stepper Recipes|Negative Resist (AutoStep 200)|R3}} |
||
| |
| |
||
|A |
|A |
||
| Line 288: | Line 310: | ||
! bgcolor="#D0E7FF" align="center" |'''Anti-Reflection Coatings''' |
! bgcolor="#D0E7FF" align="center" |'''Anti-Reflection Coatings''' |
||
{{LithRecipe Table}} |
{{LithRecipe Table}} |
||
|Picomaster XF200 (Raith) |
|||
|- |
|- |
||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/33/XHRiC-Anti-Reflective-Coating.pdf XHRiC-11] |
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/33/XHRiC-Anti-Reflective-Coating.pdf XHRiC-11] |
||
| Line 302: | Line 325: | ||
| |
| |
||
| |
| |
||
|{{rl|Stepper Recipes|DUV-42P-6}} |
|{{rl|Stepper Recipes|DUV-42P-6|R3}} |
||
| |
|||
| |
| |
||
|- |
|- |
||
| Line 311: | Line 333: | ||
| |
| |
||
| |
| |
||
|{{rl|Stepper Recipes|DS-K101-304}} |
|{{rl|Stepper Recipes|DS-K101-304|R3}} |
||
| |
| |
||
|- |
|- |
||
! bgcolor="#D0E7FF" align="center" | |
! bgcolor="#D0E7FF" align="center" | |
||
{{LithRecipe Table}} |
{{LithRecipe Table}} |
||
|Picomaster XF200 (Raith) |
|||
|} |
|} |
||
<!-- end Litho Recipes table --> |
<!-- end Litho Recipes table --> |
||
==='''Process Ranking Table'''=== |
|||
Processes in the table above are ranked by their "''Process Maturity Level''" as follows: |
|||
{| class="wikitable" |
|||
!Process Level |
|||
! colspan="11" |Description of Process Level Ranking |
|||
|- |
|||
|A |
|||
| colspan="11" |Process '''A'''llowed and materials available but never done |
|||
|- |
|||
|R1 |
|||
| colspan="11" |Process has been ran at least once |
|||
|- |
|||
|R2 |
|||
| colspan="11" |Process has been ran and procedure is documented |
|||
|- |
|||
|R3 |
|||
| colspan="11" |Process has been ran, procedure is documented, and data is available |
|||
|- |
|||
|R4 |
|||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''no''' in-Situ control available |
|||
|- |
|||
|R5 |
|||
| colspan="11" |Process has a documented procedure with regular (≥4x per year) data '''and''' in-Situ control available |
|||
|- |
|||
|R6 |
|||
| colspan="11" |Process has a documented procedure and control charts/limits available. Controlled process. |
|||
|} |
|||
==Lift-Off Recipes== |
==Lift-Off Recipes== |
||
| Line 329: | Line 379: | ||
*{{fl|Bi-LayerContactprocesswithPMGI.pdf|I-Line Lift-Off: Bi-Layer Process with PMGI Underlayer and Contact Aligner}} |
*{{fl|Bi-LayerContactprocesswithPMGI.pdf|I-Line Lift-Off: Bi-Layer Process with PMGI Underlayer and Contact Aligner}} |
||
**''Multiple processes for Metal thicknesses ~800nm to ~2.5µm'' |
**''Multiple processes for Metal thicknesses ~800nm to ~2.5µm'' |
||
**''Uses multiple DUV Flood exposure/develop cycles to create undercut.'' |
**''Uses multiple [[DUV Flood Expose|DUV Flood exposure]]/develop cycles to create undercut.'' |
||
**''Can be transferred to other I-Line litho tools (Stepper, MLA etc.)'' |
**''Can be transferred to other I-Line litho tools (Stepper, MLA etc.)'' |
||
**<u>Updates to the process:</u> |
|||
***You now only need to do 5min [[DUV Flood Expose|DUV Flood exposure]] each cycle (lamp optics were replaced) |
|||
***Use the new "101B" developer, which replaced the "SAL/101A" developers but works the same. |
|||
**There are 2 [[DUV Flood Expose|DUV Flood exposure]] + 101B develop steps because the first exposure doesn't expose the entire PMGI - because PMGI absorbs DUV very strongly so the light doesn't penetrate to the bottom of thick PMGI on the first exposure. |
|||
*[[Lift-off DUV Lift-off: LOR Underlayers|DUV Lift-off: LOR Underlayers]] |
|||
**1µm (LOR-10A) & 2-3µm (LOR-30C) versions |
|||
**Written for ASML DUV Stepper, but should work for any Imaging (top) resist, incl. I-Line tools. |
|||
*[[Lift-Off with DUV Imaging + PMGI Underlayer|DUV Lift-Off: UV6 Imaging Resist + PMGI Underlayer]] |
*[[Lift-Off with DUV Imaging + PMGI Underlayer|DUV Lift-Off: UV6 Imaging Resist + PMGI Underlayer]] |
||
**''Single-expose/develop process'' |
**''Single-expose/develop process'' |
||
| Line 348: | Line 405: | ||
===Available Variations=== |
===Available Variations=== |
||
*We have different recipes with varyious UV6 spin speeds - the same spin speed optionss as found on our manual Headway spinners. This allows for PR thickness control. See the linked UV6 datasheets below for thickness vs. rpm spin curves. |
*We have different recipes with varyious UV6 spin speeds - the same spin speed optionss as found on our manual Headway spinners. This allows for PR thickness control. See the linked UV6 datasheets below for thickness vs. rpm spin curves. '''Note''' that exact spin RPM may be slightly different between Headway spinners (on benches) vs. S-Cubed. |
||
*DSK is recommended to be spun at 1.5krpm (~40nm) for best anti-reflection properties. 5krpm (~20nm) recipes are also provided for historical/legacy processes. |
*DSK is recommended to be spun at 1.5krpm (~40nm) for best anti-reflection properties. 5krpm (~20nm) recipes are also provided for historical/legacy processes. |
||
*DSK can be baked at either 220C to act as a Dry-etchable BARC (similar to DUV-42P), or at lower temps as a developable BARC (no dry etch required). |
*DSK can be baked at either 220C to act as a Dry-etchable BARC (similar to DUV-42P), or at lower temps as a developable BARC (no dry etch required). |
||
*"Chain" recipes (with DSK+UV6 spin/cured in succession) are only available for DSK Baked at 185C & 220C, and all UV6 Spin-speed variations. For the other DSK temps you can use the single-PR "Routes". |
*"Chain" recipes (with DSK+UV6 spin/cured in succession) are only available for DSK Baked at 185C & 220C, and all UV6 Spin-speed variations. For the other DSK temps you can use the single-PR "Routes". |
||
*Developer recipes are now available for 300 MiF Developer. '''Note''' that developer is flowing continuously during the develop, so <u>develop times are shorter by ~50%</u> compared to beaker developing. |
|||
**'''DO NOT EDIT developer recipes''', they can damage the tool when programmed incorrectly! |
|||
*"Chain" recipes for 135*C Post-exposure Bake + Develop have been made. |
|||
*ASML cassettes can be placed directly on this tool for spin / exposure / develop process. Please make sure all cassettes are kept back at their respecting tools when done. |
|||
===Recipes Table (S-Cubed Flexi)=== |
===Recipes Table (S-Cubed Flexi)=== |
||
| Line 372: | Line 433: | ||
|Route |
|Route |
||
| colspan="4" |To pre-set the DSK Hotplate temp (HP4). |
| colspan="4" |To pre-set the DSK Hotplate temp (HP4). |
||
Note: Only HP4 can be changed. |
Note: Only HP4 can be changed. |
||
HP1-HP3 remains fixed at: HP1=135°C, HP2=170°C & HP3=170°C |
|||
|- |
|- |
||
| |
| |
||
| |
| |
||
|HP4-SET-220C |
|HP4-SET-'''220C''' |
||
| |
| |
||
|220°C |
|220°C |
||
| |
|Will over shoot +-2°C when done. |
||
|- |
|- |
||
| |
| |
||
| |
| |
||
|HP4-SET-210C |
|HP4-SET-'''210C''' |
||
| |
| |
||
|210°C |
|210°C |
||
| Line 390: | Line 453: | ||
| |
| |
||
| |
| |
||
|HP4-SET-200C |
|HP4-SET-'''200C''' |
||
| |
| |
||
|200°C |
|200°C |
||
| Line 397: | Line 460: | ||
| |
| |
||
| |
| |
||
|HP4-SET-185C |
|HP4-SET-'''185C''' |
||
| |
| |
||
|185 |
|185°C |
||
| |
| |
||
|- |
|- |
||
| colspan="6" |'''<u>''Bottom Anti-Reflection Coating (BARC), DSK101 only:''</u>''' |
|||
| colspan="6" | |
|||
|- |
|- |
||
|'''''[https://wiki.nanotech.ucsb.edu/wiki/images/a/af/DS-K101-304-Anti-Reflective-Coating.pdf DS-K101]''''' |
|'''''[https://wiki.nanotech.ucsb.edu/wiki/images/a/af/DS-K101-304-Anti-Reflective-Coating.pdf DS-K101]''''' |
||
| Line 408: | Line 471: | ||
| colspan="4" |''DSK101 Develop Rate depends on Bake temp - you can use this to control undercut.'' ''See: [[DS-K101-304 Bake Temp. versus Develop Rate|DSK Bake vs. Dev rate]]'' |
| colspan="4" |''DSK101 Develop Rate depends on Bake temp - you can use this to control undercut.'' ''See: [[DS-K101-304 Bake Temp. versus Develop Rate|DSK Bake vs. Dev rate]]'' |
||
DSK101 spun at 1.5K is equivalent to DUV-42P. See: [[Stepper Recipes#Anti-Reflective Coatings]] |
DSK101 spun at 1.5K is equivalent to DUV-42P. See: [[Stepper Recipes#Anti-Reflective Coatings]] |
||
'''185°C bake''' allows the DSK to dissolve during develop, and allows for undercut (may lift-off small features) |
|||
'''220°C bake''' allows DSK to be used as dry-etchable BARC (equiv. to DUV42P), requiring O2 etch to remove. Better for small features. See [[Stepper Recipes#Anti-Reflective Coatings|here for relevant processing info from DUV42P]]. |
|||
'''Note: All PR coat recipes have EBR backside clean steps included in the recipe.''' |
'''Note: All PR coat recipes have EBR backside clean steps included in the recipe.''' |
||
|- |
|- |
||
|1.5krpm recipes |
|''<u>1.5krpm</u> recipes'' |
||
| |
| |
||
|COAT-DSK101-304[1.5K]-185C |
|COAT-DSK101-304[1.5K]-'''185C''' |
||
|1.5krpm |
|1.5krpm |
||
|185°C |
|185°C |
||
| Line 420: | Line 487: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101-304[1.5K]-200C |
|COAT-DSK101-304[1.5K]-'''200C''' |
||
|1.5krpm |
|1.5krpm |
||
|200°C |
|200°C |
||
| Line 427: | Line 494: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101-304[1.5K]-210C |
|COAT-DSK101-304[1.5K]-'''210C''' |
||
|1.5krpm |
|1.5krpm |
||
|210°C |
|210°C |
||
| Line 434: | Line 501: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101-304[1.5K]-220C |
|COAT-DSK101-304[1.5K]-'''220C''' |
||
|1.5krpm |
|1.5krpm |
||
|220°C |
|220°C |
||
| Line 441: | Line 508: | ||
| colspan="6" | |
| colspan="6" | |
||
|- |
|- |
||
|5krpm recipes |
|''<u>5krpm</u> recipes'' |
||
| |
| |
||
|COAT-DSK101-304[5K]-185C |
|COAT-DSK101-304[5K]-'''185C''' |
||
|5.0krpm |
|5.0krpm |
||
|185°C |
|185°C |
||
| Line 450: | Line 517: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101-304[5K]-200C |
|COAT-DSK101-304[5K]-'''200C''' |
||
|5.0krpm |
|5.0krpm |
||
|200°C |
|200°C |
||
| Line 457: | Line 524: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101-304[5K]-210C |
|COAT-DSK101-304[5K]-'''210C''' |
||
|5.0krpm |
|5.0krpm |
||
|210°C |
|210°C |
||
| Line 464: | Line 531: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101-304[5K]-220C |
|COAT-DSK101-304[5K]-'''220C''' |
||
|5.0krpm |
|5.0krpm |
||
|220°C |
|220°C |
||
|Requires: HP4=220°C, |
|Requires: HP4=220°C, |
||
|- |
|- |
||
| colspan="6" | |
| colspan="6" |'''<u>''Imaging resist (UV6) only:''</u>''' |
||
|- |
|- |
||
|'''''[https://wiki.nanofab.ucsb.edu/w/images/3/38/UV6-Positive-Resist-Datasheet.pdf UV6-0.8]''''' |
|'''''[https://wiki.nanofab.ucsb.edu/w/images/3/38/UV6-Positive-Resist-Datasheet.pdf UV6-0.8]''''' |
||
|Route |
|Route |
||
|COAT-UV6[2K]-135C |
|COAT-UV6['''2K''']-135C |
||
|2.0krpm |
|2.0krpm |
||
|135°C |
|135°C |
||
|Requires: HP1=135°C |
|Requires: HP1=135°C |
||
|- |
|- |
||
|varying spin speed |
|''varying spin speed'' |
||
| |
| |
||
|COAT-UV6[2.5K]-135C |
|COAT-UV6['''2.5K''']-135C |
||
|2.5krpm |
|2.5krpm |
||
|135°C |
|135°C |
||
| Line 487: | Line 554: | ||
| |
| |
||
| |
| |
||
|COAT-UV6[3K]-135C |
|COAT-UV6['''3K''']-135C |
||
|3.0krpm |
|3.0krpm |
||
|135°C |
|135°C |
||
| Line 494: | Line 561: | ||
| |
| |
||
| |
| |
||
|COAT-UV6[3.5K]-135C |
|COAT-UV6['''3.5K''']-135C |
||
|3.5krpm |
|3.5krpm |
||
|135°C |
|135°C |
||
| Line 501: | Line 568: | ||
| |
| |
||
| |
| |
||
|COAT-UV6[4K]-135C |
|COAT-UV6['''4K''']-135C |
||
|4.0krpm |
|4.0krpm |
||
|135°C |
|135°C |
||
| Line 508: | Line 575: | ||
| |
| |
||
| |
| |
||
|COAT-UV6[5K]-135C |
|COAT-UV6['''5K''']-135C |
||
|5.0krpm |
|5.0krpm |
||
|135°C |
|135°C |
||
| Line 515: | Line 582: | ||
| |
| |
||
| |
| |
||
|COAT-UV6[6K]-135C |
|COAT-UV6['''6K''']-135C |
||
|6.0krpm |
|6.0krpm |
||
|135°C |
|135°C |
||
| Line 525: | Line 592: | ||
'''''+ UV6''''' |
'''''+ UV6''''' |
||
|Chain |
|Chain |
||
|COAT-DSK101[1.5K]-185C-UV6[2K]-135C |
|COAT-DSK101['''1.5K''']-185C-UV6['''2K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 2.0krpm |
UV6: 2.0krpm |
||
| Line 537: | Line 604: | ||
Plan for ~10-15 min per wafer. |
Plan for ~10-15 min per wafer. |
||
|- |
|- |
||
|1.5krpm DSK recipes with |
|''<u>1.5krpm DSK</u> recipes with'' |
||
UV6- various spin speeds |
''UV6- various spin speeds'' |
||
| |
| |
||
|COAT-DSK101[1.5K]-185C-UV6[2.5K]-135C |
|COAT-DSK101['''1.5K''']-185C-UV6['''2.5K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 2.5krpm |
UV6: 2.5krpm |
||
| Line 548: | Line 615: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[1.5K]-185C-UV6[3K]-135C |
|COAT-DSK101['''1.5K''']-185C-UV6['''3K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 3.0krpm |
UV6: 3.0krpm |
||
| Line 556: | Line 623: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[1.5K]-185C-UV6[3.5K]-135C |
|COAT-DSK101['''1.5K''']-185C-UV6['''3.5K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 3.5krpm |
UV6: 3.5krpm |
||
| Line 564: | Line 631: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[1.5K]-185C-UV6[4K]-135C |
|COAT-DSK101['''1.5K''']-185C-UV6['''4K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 4.0krpm |
UV6: 4.0krpm |
||
| Line 572: | Line 639: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[1.5K]-185C-UV6[5K]-135C |
|COAT-DSK101['''1.5K''']-185C-UV6['''5K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 5.0krpm |
UV6: 5.0krpm |
||
| Line 580: | Line 647: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[1.5K]-185C-UV6[6K]-135C |
|COAT-DSK101['''1.5K''']-185C-UV6['''6K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 6.0krpm |
UV6: 6.0krpm |
||
| Line 588: | Line 655: | ||
| colspan="6" | |
| colspan="6" | |
||
|- |
|- |
||
|5krpm DSK recipes with |
|''<u>5krpm DSK</u> recipes with'' |
||
UV6- various spin speeds |
''UV6- various spin speeds'' |
||
| |
| |
||
|COAT-DSK101[5K]-185C-UV6[2K]-135C |
|COAT-DSK101['''5K''']-185C-UV6['''2K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 2.0krpm |
UV6: 2.0krpm |
||
| Line 599: | Line 666: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-185C-UV6[2.5K]-135C |
|COAT-DSK101['''5K''']-185C-UV6['''2.5K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 2.5krpm |
UV6: 2.5krpm |
||
| Line 607: | Line 674: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-185C-UV6[3K]-135C |
|COAT-DSK101['''5K''']-185C-UV6['''3K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 3.0krpm |
UV6: 3.0krpm |
||
| Line 615: | Line 682: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-185C-UV6[3.5K]-135C |
|COAT-DSK101['''5K''']-185C-UV6['''3.5K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 3.5krpm |
UV6: 3.5krpm |
||
| Line 623: | Line 690: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-185C-UV6[4K]-135C |
|COAT-DSK101['''5K''']-185C-UV6['''4K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 4.0krpm |
UV6: 4.0krpm |
||
| Line 631: | Line 698: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-185C-UV6[5K]-135C |
|COAT-DSK101['''5K''']-185C-UV6['''5K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 5.0krpm |
UV6: 5.0krpm |
||
| Line 639: | Line 706: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-185C-UV6[6K]-135C |
|COAT-DSK101['''5K''']-185C-UV6['''6K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 6.0krpm |
UV6: 6.0krpm |
||
| Line 650: | Line 717: | ||
'''''+ UV6''''' |
'''''+ UV6''''' |
||
|Chain |
|Chain |
||
|COAT-DSK101[1.5K]-220C-UV6[2K]-135C |
|COAT-DSK101['''1.5K''']-220C-UV6['''2K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 2.0krpm |
UV6: 2.0krpm |
||
| Line 662: | Line 729: | ||
Plan for ~10-15 min per wafer. |
Plan for ~10-15 min per wafer. |
||
|- |
|- |
||
|1.5krpm DSK recipes with |
|''<u>1.5krpm DSK</u> recipes with'' |
||
UV6- various spin speeds |
''UV6- various spin speeds'' |
||
| |
| |
||
|COAT-DSK101[1.5K]-220C-UV6[2.5K]-135C |
|COAT-DSK101['''1.5K''']-220C-UV6['''2.5K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 2.5krpm |
UV6: 2.5krpm |
||
| Line 673: | Line 740: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[1.5K]-220C-UV6[3K]-135C |
|COAT-DSK101['''1.5K''']-220C-UV6['''3K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 3.0krpm |
UV6: 3.0krpm |
||
| Line 681: | Line 748: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[1.5K]-220C-UV6[3.5K]-135C |
|COAT-DSK101['''1.5K''']-220C-UV6['''3.5K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 3.5krpm |
UV6: 3.5krpm |
||
| Line 689: | Line 756: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[1.5K]-220C-UV6[4K]-135C |
|COAT-DSK101['''1.5K''']-220C-UV6['''4K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 4.0krpm |
UV6: 4.0krpm |
||
| Line 697: | Line 764: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[1.5K]-220C-UV6[5K]-135C |
|COAT-DSK101['''1.5K''']-220C-UV6['''5K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 5.0krpm |
UV6: 5.0krpm |
||
| Line 705: | Line 772: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[1.5K]-220C-UV6[6K]-135C |
|COAT-DSK101['''1.5K''']-220C-UV6['''6K''']-135C |
||
|DSK: 1.5krpm |
|DSK: 1.5krpm |
||
UV6: 6.0krpm |
UV6: 6.0krpm |
||
| Line 713: | Line 780: | ||
| colspan="6" | |
| colspan="6" | |
||
|- |
|- |
||
|5krpm DSK recipes with |
|''<u>5krpm DSK</u> recipes with'' |
||
UV6- various spin speeds |
''UV6- various spin speeds'' |
||
| |
| |
||
|COAT-DSK101[5K]-220C-UV6[2K]-135C |
|COAT-DSK101['''5K''']-220C-UV6['''2K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 2.0krpm |
UV6: 2.0krpm |
||
| Line 724: | Line 791: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-220C-UV6[2.5K]-135C |
|COAT-DSK101['''5K''']-220C-UV6['''2.5K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 2.5krpm |
UV6: 2.5krpm |
||
| Line 732: | Line 799: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-220C-UV6[3K]-135C |
|COAT-DSK101['''5K''']-220C-UV6['''3K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 3.0krpm |
UV6: 3.0krpm |
||
| Line 740: | Line 807: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-220C-UV6[3.5K]-135C |
|COAT-DSK101['''5K''']-220C-UV6['''3.5K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 3.5krpm |
UV6: 3.5krpm |
||
| Line 748: | Line 815: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-220C-UV6[4K]-135C |
|COAT-DSK101['''5K''']-220C-UV6['''4K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 4.0krpm |
UV6: 4.0krpm |
||
| Line 756: | Line 823: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-220C-UV6[5K]-135C |
|COAT-DSK101['''5K''']-220C-UV6['''5K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 5.0krpm |
UV6: 5.0krpm |
||
| Line 764: | Line 831: | ||
| |
| |
||
| |
| |
||
|COAT-DSK101[5K]-220C-UV6[6K]-135C |
|COAT-DSK101['''5K''']-220C-UV6['''6K''']-135C |
||
|DSK: 5krpm |
|DSK: 5krpm |
||
UV6: 6.0krpm |
UV6: 6.0krpm |
||
| Line 791: | Line 858: | ||
|'''''PEB and Developing''''' |
|'''''PEB and Developing''''' |
||
|Route |
|Route |
||
| colspan="4" |To bake wafer |
| colspan="4" |To post-exposure bake wafer after exposure (std. PEB for UV6) 90sec, cool 15sec, develop using AZ300MIF and water rinse 60sec |
||
WARNING: |
'''WARNING''': DO NOT USE ANY OTHER DEVELOPER RECIPES OTHER THAN THE ONES LISTED HERE (or equipment damage may occur!) |
||
|- |
|- |
||
|Varying developer time |
|''Varying developer time'' |
||
| |
| |
||
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-10S |
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-'''10S''' |
||
|Developer chuck: 300rpm |
|Developer chuck: 300rpm |
||
|135°C |
|135°C |
||
| Line 804: | Line 871: | ||
| |
| |
||
| |
| |
||
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-15S |
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-'''15S''' |
||
|same as above |
|same as above |
||
|same as above |
|same as above |
||
| Line 811: | Line 878: | ||
| |
| |
||
| |
| |
||
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-20S |
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-'''20S''' |
||
|same as above |
|||
|same as above |
|||
|same as above |
|||
|- |
|||
| |
|||
| |
|||
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-'''25S''' |
|||
|same as above |
|||
|same as above |
|||
|same as above |
|||
|- |
|||
| |
|||
| |
|||
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-'''30S''' |
|||
|same as above |
|||
|same as above |
|||
|same as above |
|||
|- |
|||
| |
|||
| |
|||
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-'''35S''' |
|||
|same as above |
|||
|same as above |
|||
|same as above |
|||
|- |
|||
| |
|||
| |
|||
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-'''40S''' |
|||
|same as above |
|||
|same as above |
|||
|same as above |
|||
|- |
|||
| |
|||
| |
|||
|BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-'''45S''' |
|||
|same as above |
|same as above |
||
|same as above |
|same as above |
||
| Line 820: | Line 922: | ||
|'''Developing''' |
|'''Developing''' |
||
|Route |
|Route |
||
| colspan="4" |To only develop wafer using AZ300MIF and water rinse 60sec |
| colspan="4" |To only develop wafer using AZ300MIF and water rinse 60sec (No PEB) |
||
WARNING: |
'''WARNING''': DO NOT USE ANY OTHER DEVELOPER RECIPES OTHER THAN THE ONES LISTED HERE (or equipment damage may occur!) |
||
|- |
|- |
||
|Varying developer time |
|''Varying developer time'' |
||
| |
| |
||
|DEV[MIF300]-SPIN[300RPM]-10S |
|DEV[MIF300]-SPIN[300RPM]-'''10S''' |
||
|Developer chuck: 300rpm |
|Developer chuck: 300rpm |
||
|135°C |
|135°C |
||
| Line 833: | Line 935: | ||
| |
| |
||
| |
| |
||
|DEV[MIF300]-SPIN[300RPM]-15S |
|DEV[MIF300]-SPIN[300RPM]-'''15S''' |
||
|same as above |
|same as above |
||
|same as above |
|same as above |
||
| Line 840: | Line 942: | ||
| |
| |
||
| |
| |
||
|DEV[MIF300]-SPIN[300RPM]-20S |
|DEV[MIF300]-SPIN[300RPM]-'''20S''' |
||
|same as above |
|||
|same as above |
|||
|same as above |
|||
|- |
|||
| |
|||
| |
|||
|DEV[MIF300]-SPIN[300RPM]-'''25S''' |
|||
|same as above |
|||
|same as above |
|||
|same as above |
|||
|- |
|||
| |
|||
| |
|||
|DEV[MIF300]-SPIN[300RPM]-'''30S''' |
|||
|same as above |
|||
|same as above |
|||
|same as above |
|||
|- |
|||
| |
|||
| |
|||
|DEV[MIF300]-SPIN[300RPM]-'''35S''' |
|||
|same as above |
|||
|same as above |
|||
|same as above |
|||
|- |
|||
| |
|||
| |
|||
|DEV[MIF300]-SPIN[300RPM]-'''40S''' |
|||
|same as above |
|||
|same as above |
|||
|same as above |
|||
|- |
|||
| |
|||
| |
|||
|DEV[MIF300]-SPIN[300RPM]-'''45S''' |
|||
|same as above |
|same as above |
||
|same as above |
|same as above |
||
| Line 868: | Line 1,005: | ||
==Chemicals Stocked + Datasheets== |
==Chemicals Stocked + Datasheets== |
||
''The following is a list of the lithography chemicals we stock in the lab, with links to the datasheets for each. The datasheets will often have important processing info such as spin-speed vs. thickness curves, typical process parameters, bake temps/times etc.'' |
''The following is a list of the lithography chemicals we stock in the lab, with links to the datasheets for each. The datasheets will often have important processing info such as spin-speed vs. thickness curves, typical process parameters, bake temps/times etc.'' |
||
Item numbers in (parentheses) indicate the specific stocked formulation, when the datasheet shows multiple formulations. |
|||
{| |
{| |
||
|- valign="top" |
|- valign="top" |
||
| Line 909: | Line 1,048: | ||
;<div id="Underlayers"><big>Underlayers</big></div> |
;<div id="Underlayers"><big>Underlayers</big></div> |
||
See [[Lithography Recipes#Lift-Off Recipes|this page for lift-off recipes.]] |
|||
*{{fl|PMGI-Underlayer-Datasheet.pdf|PMGI (PMGI SF3,5,8,11,15)}} |
*{{fl|PMGI-Underlayer-Datasheet.pdf|PMGI (PMGI SF3,5,8,11,15)}} |
||
*LOR ([[Media:Lor pds.pdf|LOR 10A & LOR 30C]]) |
|||
*{{fl|LOL2000-Underlayer-Datasheet.pdf|Shipley LOL2000}} |
*{{fl|LOL2000-Underlayer-Datasheet.pdf|Shipley LOL2000}} |
||
| Line 948: | Line 1,088: | ||
*{{fl|BCB-cyclotene-3000-revA.pdf|BCB, Cyclotene 3022-46(Not Photosensitive)}} |
*{{fl|BCB-cyclotene-3000-revA.pdf|BCB, Cyclotene 3022-46(Not Photosensitive)}} |
||
*{{fl|BCB-cyclotene-4000-revA.pdf|PhotoBCB, Cyclotene |
*{{fl|BCB-cyclotene-4000-revA.pdf|PhotoBCB, Cyclotene 4024-40(Negative Polarity)}} |
||
*{{fl|BCB-adhesion.pdf|BCB Adhesion Notes from Vendor}} |
*{{fl|BCB-adhesion.pdf|BCB Adhesion Notes from Vendor}} |
||
*{{fl|BCB-rework.pdf|BCB rework Notes from Vendor}} |
*{{fl|BCB-rework.pdf|BCB rework Notes from Vendor}} |
||
*{{fl|512B-Datasheet-revA.pdf|Spin-on-Glass, Honeywell 512B (Not Photosensitive)}} |
|||
*{{fl|512B-Application-Data-Bake-revA.pdf|Honeywell 512B Apps Data}} |
|||
;<div id="Developers"><big>Developers</big></div> |
;<div id="Developers"><big>Developers</big></div> |
||
Latest revision as of 22:43, 22 October 2026
| Table of Contents |
|---|
Photolithography Processes
|
Photolithography Chemicals/Materials
|
General Photolithography Techniques
HMDS Process for Improving Adhesion
- Use these procedures if you are finding poor adhesion PR lifting-off), or for chemicals (like BHF) that attack the PR adhesion interface strongly.
Edge-Bead Removal Techniques
- These techniques are required for loading full-wafers into etchers that use top-side clamps, to prevent photoresist from sticking to the clamp (and potentially destroying your wafer).
- For contact lithography, this improves the proximity of the mask plate and sample, improving resolution. For some projection systems, such as the Maskless Aligner, EBR can help with autofocus issues.
- For small samples (<1cm) some techniques here to reduce edge-bead via shims.
Photoresist reflow (MicroChem)
- To create slanted sidewalls or curved surfaces.
Lithography Calibration - Analyzing a Focus-Exposure Matrix
- On tools with autofocus (steppers & direct-write litho tools), you calibrate your litho by shooting a "Focus Exposure Matrix/Array", or "FEM/FEA", which exposes a grid with Dose varying in one axis, and Focus varying in the other.
- Explains how to locate the "Process Window" for your lithography.
Photolithography Recipes
Process Maturity Ranking
R6- most mature process with regular calibrations recorded on SPC charts.- …
R1- least mature - "possible" but you'll have to figure it out.A: Material is available for use, but no recipes are provided.
The Key/Legend for this table's R1...R6 values is at the bottom of the table.
Click the tool title to go to recipes for that tool.
Click the photoresist title to get the datasheet, also found in Stocked Chemicals + Datasheets.
Process Ranking Table
Processes in the table above are ranked by their "Process Maturity Level" as follows:
| Process Level | Description of Process Level Ranking | ||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|
| A | Process Allowed and materials available but never done | ||||||||||
| R1 | Process has been ran at least once | ||||||||||
| R2 | Process has been ran and procedure is documented | ||||||||||
| R3 | Process has been ran, procedure is documented, and data is available | ||||||||||
| R4 | Process has a documented procedure with regular (≥4x per year) data no in-Situ control available | ||||||||||
| R5 | Process has a documented procedure with regular (≥4x per year) data and in-Situ control available | ||||||||||
| R6 | Process has a documented procedure and control charts/limits available. Controlled process. | ||||||||||
Lift-Off Recipes
- Lift-Off Description/Tutorial
- How it works, process limits and considerations for designing your process
- I-Line Lift-Off: Bi-Layer Process with LOL2000 Underlayer
- Single Expose/Develop process for simplicity
- Up to ~130nm metal thickness & ≥500nm-1000nm gap between metal.
- Can use any I-Line litho tool (GCA Stepper, Contact aligner, MLA)
- I-Line Lift-Off: Bi-Layer Process with PMGI Underlayer and Contact Aligner
- Multiple processes for Metal thicknesses ~800nm to ~2.5µm
- Uses multiple DUV Flood exposure/develop cycles to create undercut.
- Can be transferred to other I-Line litho tools (Stepper, MLA etc.)
- Updates to the process:
- You now only need to do 5min DUV Flood exposure each cycle (lamp optics were replaced)
- Use the new "101B" developer, which replaced the "SAL/101A" developers but works the same.
- There are 2 DUV Flood exposure + 101B develop steps because the first exposure doesn't expose the entire PMGI - because PMGI absorbs DUV very strongly so the light doesn't penetrate to the bottom of thick PMGI on the first exposure.
- DUV Lift-off: LOR Underlayers
- 1µm (LOR-10A) & 2-3µm (LOR-30C) versions
- Written for ASML DUV Stepper, but should work for any Imaging (top) resist, incl. I-Line tools.
- DUV Lift-Off: UV6 Imaging Resist + PMGI Underlayer
- Single-expose/develop process
- Up to ~65nm metal thickness & ~350nm gap between metal
- Use thicker PMGI for thicker metals
E-Beam Lithography Recipes (JEOL JBX-6300FS)
- Under Development.
FIB Lithography Recipes (Raith Velion)
To Be Added
Automated Coat/Develop System Recipes (S-Cubed Flexi)
Recipes pre-loaded on the S-Cubed Flexi automated coat/bake/develop system. Only staff may write new recipes, contact the tool supervisor for more info.
Available Variations
- We have different recipes with varyious UV6 spin speeds - the same spin speed optionss as found on our manual Headway spinners. This allows for PR thickness control. See the linked UV6 datasheets below for thickness vs. rpm spin curves. Note that exact spin RPM may be slightly different between Headway spinners (on benches) vs. S-Cubed.
- DSK is recommended to be spun at 1.5krpm (~40nm) for best anti-reflection properties. 5krpm (~20nm) recipes are also provided for historical/legacy processes.
- DSK can be baked at either 220C to act as a Dry-etchable BARC (similar to DUV-42P), or at lower temps as a developable BARC (no dry etch required).
- "Chain" recipes (with DSK+UV6 spin/cured in succession) are only available for DSK Baked at 185C & 220C, and all UV6 Spin-speed variations. For the other DSK temps you can use the single-PR "Routes".
- Developer recipes are now available for 300 MiF Developer. Note that developer is flowing continuously during the develop, so develop times are shorter by ~50% compared to beaker developing.
- DO NOT EDIT developer recipes, they can damage the tool when programmed incorrectly!
- "Chain" recipes for 135*C Post-exposure Bake + Develop have been made.
- ASML cassettes can be placed directly on this tool for spin / exposure / develop process. Please make sure all cassettes are kept back at their respecting tools when done.
Recipes Table (S-Cubed Flexi)
| Coating Material | Route/Chain | Name: (User: "UCSB Users") | Spin Speed (krpm) | Bake Temp | Notes |
| BEFORE LITHOGRAPHY (PR Coat and Bake) | |||||
|---|---|---|---|---|---|
| Hotplate Set | Route | To pre-set the DSK Hotplate temp (HP4).
Note: Only HP4 can be changed. HP1-HP3 remains fixed at: HP1=135°C, HP2=170°C & HP3=170°C | |||
| HP4-SET-220C | 220°C | Will over shoot +-2°C when done. | |||
| HP4-SET-210C | 210°C | ||||
| HP4-SET-200C | 200°C | ||||
| HP4-SET-185C | 185°C | ||||
| Bottom Anti-Reflection Coating (BARC), DSK101 only: | |||||
| DS-K101 | Route | DSK101 Develop Rate depends on Bake temp - you can use this to control undercut. See: DSK Bake vs. Dev rate
DSK101 spun at 1.5K is equivalent to DUV-42P. See: Stepper Recipes#Anti-Reflective Coatings 185°C bake allows the DSK to dissolve during develop, and allows for undercut (may lift-off small features) 220°C bake allows DSK to be used as dry-etchable BARC (equiv. to DUV42P), requiring O2 etch to remove. Better for small features. See here for relevant processing info from DUV42P. Note: All PR coat recipes have EBR backside clean steps included in the recipe. | |||
| 1.5krpm recipes | COAT-DSK101-304[1.5K]-185C | 1.5krpm | 185°C | Requires: HP4=185°C, | |
| COAT-DSK101-304[1.5K]-200C | 1.5krpm | 200°C | Requires: HP4=200°C | ||
| COAT-DSK101-304[1.5K]-210C | 1.5krpm | 210°C | Requires: HP4=210°C | ||
| COAT-DSK101-304[1.5K]-220C | 1.5krpm | 220°C | Requires: HP4=220°C, | ||
| 5krpm recipes | COAT-DSK101-304[5K]-185C | 5.0krpm | 185°C | Requires: HP4=185°C, | |
| COAT-DSK101-304[5K]-200C | 5.0krpm | 200°C | Requires: HP4=200°C | ||
| COAT-DSK101-304[5K]-210C | 5.0krpm | 210°C | Requires: HP4=210°C | ||
| COAT-DSK101-304[5K]-220C | 5.0krpm | 220°C | Requires: HP4=220°C, | ||
| Imaging resist (UV6) only: | |||||
| UV6-0.8 | Route | COAT-UV6[2K]-135C | 2.0krpm | 135°C | Requires: HP1=135°C |
| varying spin speed | COAT-UV6[2.5K]-135C | 2.5krpm | 135°C | Requires: HP1=135°C | |
| COAT-UV6[3K]-135C | 3.0krpm | 135°C | Requires: HP1=135°C | ||
| COAT-UV6[3.5K]-135C | 3.5krpm | 135°C | Requires: HP1=135°C | ||
| COAT-UV6[4K]-135C | 4.0krpm | 135°C | Requires: HP1=135°C | ||
| COAT-UV6[5K]-135C | 5.0krpm | 135°C | Requires: HP1=135°C | ||
| COAT-UV6[6K]-135C | 6.0krpm | 135°C | Requires: HP1=135°C | ||
| UV6 Coat with Developable BARC underlayer: | |||||
| DS-K101 @ 185°C
+ UV6 |
Chain | COAT-DSK101[1.5K]-185C-UV6[2K]-135C | DSK: 1.5krpm
UV6: 2.0krpm |
DSK: 185°C
UV6: 135°C |
Requires:
– HP4=185°C – HP1=135°C Plan for ~10-15 min per wafer. |
| 1.5krpm DSK recipes with
UV6- various spin speeds |
COAT-DSK101[1.5K]-185C-UV6[2.5K]-135C | DSK: 1.5krpm
UV6: 2.5krpm |
same as above | same as above | |
| COAT-DSK101[1.5K]-185C-UV6[3K]-135C | DSK: 1.5krpm
UV6: 3.0krpm |
same as above | same as above | ||
| COAT-DSK101[1.5K]-185C-UV6[3.5K]-135C | DSK: 1.5krpm
UV6: 3.5krpm |
same as above | same as above | ||
| COAT-DSK101[1.5K]-185C-UV6[4K]-135C | DSK: 1.5krpm
UV6: 4.0krpm |
same as above | same as above | ||
| COAT-DSK101[1.5K]-185C-UV6[5K]-135C | DSK: 1.5krpm
UV6: 5.0krpm |
same as above | same as above | ||
| COAT-DSK101[1.5K]-185C-UV6[6K]-135C | DSK: 1.5krpm
UV6: 6.0krpm |
same as above | same as above | ||
| 5krpm DSK recipes with
UV6- various spin speeds |
COAT-DSK101[5K]-185C-UV6[2K]-135C | DSK: 5krpm
UV6: 2.0krpm |
same as above | same as above | |
| COAT-DSK101[5K]-185C-UV6[2.5K]-135C | DSK: 5krpm
UV6: 2.5krpm |
same as above | same as above | ||
| COAT-DSK101[5K]-185C-UV6[3K]-135C | DSK: 5krpm
UV6: 3.0krpm |
same as above | same as above | ||
| COAT-DSK101[5K]-185C-UV6[3.5K]-135C | DSK: 5krpm
UV6: 3.5krpm |
same as above | same as above | ||
| COAT-DSK101[5K]-185C-UV6[4K]-135C | DSK: 5krpm
UV6: 4.0krpm |
same as above | same as above | ||
| COAT-DSK101[5K]-185C-UV6[5K]-135C | DSK: 5krpm
UV6: 5.0krpm |
same as above | same as above | ||
| COAT-DSK101[5K]-185C-UV6[6K]-135C | DSK: 5krpm
UV6: 6.0krpm |
same as above | same as above | ||
| UV6 Coat with Dry-Etchable BARC underlayer: | |||||
| DS-K101 @ 220°C
+ UV6 |
Chain | COAT-DSK101[1.5K]-220C-UV6[2K]-135C | DSK: 1.5krpm
UV6: 2.0krpm |
DSK: 220°C
UV6: 135°C |
Requires:
– HP4=220°C – HP1=135°C Plan for ~10-15 min per wafer. |
| 1.5krpm DSK recipes with
UV6- various spin speeds |
COAT-DSK101[1.5K]-220C-UV6[2.5K]-135C | DSK: 1.5krpm
UV6: 2.5krpm |
same as above | same as above | |
| COAT-DSK101[1.5K]-220C-UV6[3K]-135C | DSK: 1.5krpm
UV6: 3.0krpm |
same as above | same as above | ||
| COAT-DSK101[1.5K]-220C-UV6[3.5K]-135C | DSK: 1.5krpm
UV6: 3.5krpm |
same as above | same as above | ||
| COAT-DSK101[1.5K]-220C-UV6[4K]-135C | DSK: 1.5krpm
UV6: 4.0krpm |
same as above | same as above | ||
| COAT-DSK101[1.5K]-220C-UV6[5K]-135C | DSK: 1.5krpm
UV6: 5.0krpm |
same as above | same as above | ||
| COAT-DSK101[1.5K]-220C-UV6[6K]-135C | DSK: 1.5krpm
UV6: 6.0krpm |
same as above | same as above | ||
| 5krpm DSK recipes with
UV6- various spin speeds |
COAT-DSK101[5K]-220C-UV6[2K]-135C | DSK: 5krpm
UV6: 2.0krpm |
same as above | same as above | |
| COAT-DSK101[5K]-220C-UV6[2.5K]-135C | DSK: 5krpm
UV6: 2.5krpm |
same as above | same as above | ||
| COAT-DSK101[5K]-220C-UV6[3K]-135C | DSK: 5krpm
UV6: 3.0krpm |
same as above | same as above | ||
| COAT-DSK101[5K]-220C-UV6[3.5K]-135C | DSK: 5krpm
UV6: 3.5krpm |
same as above | same as above | ||
| COAT-DSK101[5K]-220C-UV6[4K]-135C | DSK: 5krpm
UV6: 4.0krpm |
same as above | same as above | ||
| COAT-DSK101[5K]-220C-UV6[5K]-135C | DSK: 5krpm
UV6: 5.0krpm |
same as above | same as above | ||
| COAT-DSK101[5K]-220C-UV6[6K]-135C | DSK: 5krpm
UV6: 6.0krpm |
same as above | same as above | ||
| AFTER LITHOGRAPHY (PEB and Developing) | |||||
| PEB Wafer Bake | Route | To bake wafer with UV6 after exposure (PEB) for 90sec and cool for 15sec | |||
| BAKE-135C-90S | 135°C | Requires: HP1=135°C | |||
| PEB and Developing | Route | To post-exposure bake wafer after exposure (std. PEB for UV6) 90sec, cool 15sec, develop using AZ300MIF and water rinse 60sec
WARNING: DO NOT USE ANY OTHER DEVELOPER RECIPES OTHER THAN THE ONES LISTED HERE (or equipment damage may occur!) | |||
| Varying developer time | BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-10S | Developer chuck: 300rpm | 135°C | Requires: HP1=135°C | |
| BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-15S | same as above | same as above | same as above | ||
| BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-20S | same as above | same as above | same as above | ||
| BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-25S | same as above | same as above | same as above | ||
| BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-30S | same as above | same as above | same as above | ||
| BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-35S | same as above | same as above | same as above | ||
| BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-40S | same as above | same as above | same as above | ||
| BAKE-135C-90S-DEV[MIF300]-SPIN[300RPM]-45S | same as above | same as above | same as above | ||
| Developing | Route | To only develop wafer using AZ300MIF and water rinse 60sec (No PEB)
WARNING: DO NOT USE ANY OTHER DEVELOPER RECIPES OTHER THAN THE ONES LISTED HERE (or equipment damage may occur!) | |||
| Varying developer time | DEV[MIF300]-SPIN[300RPM]-10S | Developer chuck: 300rpm | 135°C | Requires: HP1=135°C | |
| DEV[MIF300]-SPIN[300RPM]-15S | same as above | same as above | same as above | ||
| DEV[MIF300]-SPIN[300RPM]-20S | same as above | same as above | same as above | ||
| DEV[MIF300]-SPIN[300RPM]-25S | same as above | same as above | same as above | ||
| DEV[MIF300]-SPIN[300RPM]-30S | same as above | same as above | same as above | ||
| DEV[MIF300]-SPIN[300RPM]-35S | same as above | same as above | same as above | ||
| DEV[MIF300]-SPIN[300RPM]-40S | same as above | same as above | same as above | ||
| DEV[MIF300]-SPIN[300RPM]-45S | same as above | same as above | same as above | ||
Holography Recipes
The Holography recipes here use the BARC layer XHRiC-11 & the high-res. I-Line photoresist THMR-IP3600HP-D.
- Standard Holography Process - on SiO2 on Si
- Holography Process Variations - Set-up Angle - Etching into SiO2 and Si
- Etch SiO2 Nano-structure - Changing Side-wall Angle - Etching into Si with a different line-width
- Reduce SiO2 Nanowire Diameter - Thermal Oxidation - Vapor HF Etching
Low-K Spin-On Dielectric Recipes
Chemicals Stocked + Datasheets
The following is a list of the lithography chemicals we stock in the lab, with links to the datasheets for each. The datasheets will often have important processing info such as spin-speed vs. thickness curves, typical process parameters, bake temps/times etc.
Item numbers in (parentheses) indicate the specific stocked formulation, when the datasheet shows multiple formulations.