Difference between revisions of "Lithography Recipes"
(→Photolithography Recipes: deleted SPR 950-0.8 row) |
m (fixed link) |
||
(46 intermediate revisions by 4 users not shown) | |||
Line 1: | Line 1: | ||
− | + | __NOTOC__ | |
− | |||
− | |||
− | |||
{| class="wikitable" | {| class="wikitable" | ||
|+ | |+ | ||
!Table of Contents | !Table of Contents | ||
|- | |- | ||
− | |''' | + | | |
− | + | ==='''<big>Photolithography Processes</big>'''=== | |
− | **[[#Photolithography_Recipes |Photo Lithography Recipe section]] | + | |
− | + | #'''UV Optical Lithography''' | |
− | + | #*[[#PositivePR |'''Stocked Lithography Chemical + Datasheets''']] | |
− | **[[# | + | #**''Lists all stocked photolith. chemicals, PRs, strippers, developers, and links to the chemical's application notes/datasheet, which detail the spin curves and nominal processes.'' |
− | ***'' | + | #*[[#Photolithography_Recipes |'''Photo Lithography Recipe section''']] |
− | + | #**''Starting recipes (spin, bake, exposure, develop etc.) for all photolith. tools.'' | |
− | + | #**''Substrate/surface materials/pattern size can affect process parameters. Users may need to run Focus/Exposure Arrays/Matrix (FEA's/FEM's) with these processes to achieve high-resolution.'' | |
− | + | #**[[Contact Alignment Recipes|<u>Contact Aligner Recipes</u>]] | |
− | + | #***[[Contact Alignment Recipes#Suss Aligners .28SUSS MJB-3.29|Suss MJB Aligners]] | |
− | + | #***[[Contact Alignment Recipes#Contact Aligner .28SUSS MA-6.29|Suss MA6]] | |
− | + | #**[[Stepper Recipes|<u>Stepper Recipes</u>]] | |
− | + | #***[[Stepper Recipes#Stepper 1 .28GCA 6300.29|Stepper #1: GCA 6300]] (I-Line) | |
− | + | #***[[Stepper Recipes#Stepper 2 .28AutoStep 200.29|Stepper #2: GCA Autostep 200]] (I-Line) | |
− | + | #***[[Stepper Recipes#Stepper 3 .28ASML DUV.29|Stepper #3: ASML PAS 5500/300]] (DUV) | |
− | + | #**[[Direct-Write Lithography Recipes|<u>Direct-Write Recipes</u>]] | |
− | + | #***[[Direct-Write Lithography Recipes#Maskless Aligner .28Heidelberg MLA150.29|Heidelberg MLA150]] | |
− | + | #***[[Lithography Recipes#E-Beam Lithography Recipes|JEOL JBX-6300FS EBL]] | |
− | + | #***[[Lithography Recipes#FIB Lithography Recipes .28Raith Velion.29|Raith Velion FIB]] | |
− | + | #**[[Lithography Recipes#Automated Coat.2FDevelop System Recipes .28S-Cubed Flexi.29|Automated Coater Recipes (S-Cubed Flexi)]] | |
+ | #[[Lithography Recipes#General Photolithography Techniques|'''General Photolithography Techniques''']] | ||
+ | #*''Techniques for improving litho. or solving common photolith. problems.'' | ||
+ | #'''[[Lithography Recipes#Lift-Off Recipes|Lift-Off Recipes]]''' | ||
+ | #*''Verified Recipes for lift-off using various photolith. tools'' | ||
+ | #*''General educational description of this technique and it's limitations/considerations.'' | ||
+ | #'''E-beam Lithography''' | ||
+ | #*[[#E-Beam_Lithography_Recipes |E-Beam Lithography Recipes]] | ||
+ | #**''Has links to starting recipes. Substrates and patterns play a large role in process parameters.'' | ||
+ | #*[[#EBLPR |EBL Photoresist Datasheets]] | ||
+ | #**''Provided for reference, also showing starting recipes and usage info.'' | ||
+ | #'''[[Lithography Recipes#Holography Recipes|Holography]]''' | ||
+ | #*''For 1-D and 2-D gratings with 220nm nominal period, available on substrates up to 1 inch square.'' | ||
+ | #*''Recipes for silicon substrates are provided, and have been translated to other substrates by users.'' | ||
+ | #*''Datasheets are provided with starting recipes and usage info.'' | ||
+ | #'''[[Lithography Recipes#Edge-Bead Removal Techniques|Edge-Bead Removal]]''' | ||
+ | #*''Edge photoresist removal methods needed for clamp-based etchers'' | ||
+ | #*''Improves resolution for contact lithography'' | ||
+ | |- | ||
+ | | | ||
− | + | ==='''<big>Photolithography Chemicals/Materials</big>'''=== | |
− | |||
− | |||
− | |||
− | |||
− | |||
− | |||
− | |||
− | |||
− | |||
− | |||
− | |||
− | |||
− | |||
− | |||
− | *'''[[#SpinOnDielectrics |Low-K Spin-on Dielectrics]]''' | + | #'''[[#Underlayers |Underlayers]]''' |
− | + | #*''These are used beneath resists for both adhesive purposes and to enable bi-layer lift-off profiles for use with photoresist.'' | |
− | + | #*''Datasheets are provided.'' | |
− | + | #'''[[#AntiReflectionCoatings |Anti-Reflection Coatings]]''': | |
− | + | #*[[#Photolithography_Recipes |The Photoresist Recipes]] section contains recipes using these materials. | |
− | + | #*''Bottom Anti-Reflection Coatings (BARC) are used in the stepper systems, underneath the resists to eliminate substrate reflections that can affect resolution and repeatability for small, near resolution limited, feature sizes.'' | |
− | + | #*''Datasheets are provided for reference on use of the materials.'' | |
− | + | #'''[[#ContrastEnhancement |Contrast Enhancement Materials (CEM)]]''' | |
+ | #*[[#Photolithography_Recipes |The Photoresist Recipes]] section contains recipes using these materials. | ||
+ | #*''Used for resolution enhancement. Not for use in contact aligners, typically used on I-Line Steppers.'' | ||
+ | #*''Datasheets provided with usage info.'' | ||
+ | #'''[[#AdhesionPromoters |Adhesion Promoters]]''' | ||
+ | #*''These are used to improve wetting of photoresists to your substrate.'' | ||
+ | #*''Datasheets are provided on use of these materials.'' | ||
+ | #'''[[#SpinOnDielectrics |Low-K Spin-on Dielectrics]]''' | ||
+ | #*[[Lithography Recipes#SpinOnDielectrics|Spin-On Dielectrics]] | ||
+ | #**''Datasheets for BCB, Photo-BCB, and SOG (spin-on-glass) for reference on use.'' | ||
+ | #*[[#Low-K_Spin-On_Dielectric_Recipes |Low-K Spin-On Dielectric Recipes]] | ||
+ | #**''Recipes for usage of some spin-on dielectrics.'' | ||
+ | #'''[[#Developers |Developers and Removers]]''' | ||
+ | #*''Datasheets provided for reference.'' | ||
+ | #*''Remover and Photoresist Strippers are used to dissolve PR during lift-off or after etching.'' | ||
|} | |} | ||
+ | |||
+ | ==General Photolithography Techniques== | ||
+ | |||
+ | ====[[Photolithography - Improving Adhesion Photoresist Adhesion|'''HMDS Process for Improving Adhesion''']]==== | ||
+ | |||
+ | *''Use these procedures if you are finding poor adhesion PR lifting-off), or for chemicals (like BHF) that attack the PR adhesion interface strongly.'' | ||
+ | |||
+ | ====[[Photolithography - Manual Edge-Bead Removal Techniques|'''Edge-Bead Removal Techniques''']]==== | ||
+ | |||
+ | *''These techniques are required for loading full-wafers into etchers that use top-side clamps, to prevent photoresist from sticking to the clamp (and potentially destroying your wafer).'' | ||
+ | *''For contact lithography, this improves the proximity of the mask plate and sample, improving resolution. For some projection systems, such as the [[Maskless Aligner (Heidelberg MLA150)|Maskless Aligner]], EBR can help with autofocus issues.'' | ||
+ | |||
+ | ====[https://www.microchemicals.com/technical_information/reflow_photoresist.pdf '''Photoresist reflow (MicroChem)''']==== | ||
+ | |||
+ | *''To create slanted sidewalls or curved surfaces.'' | ||
==Photolithography Recipes== | ==Photolithography Recipes== | ||
− | + | *<small>'''R''': ''Recipe is available. Clicking this link will take you to the recipe.''</small> | |
+ | *<small>'''A''': ''Material is available for use, but no recipes are provided.''</small> | ||
+ | ''Click the tool title to go to recipes for that tool.'' | ||
+ | |||
+ | ''Click the photoresist title to get the datasheet, also found in [[Lithography Recipes#Chemicals Stocked .2B Datasheets|Stocked Chemicals + Datasheets]].'' | ||
{| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" | {| class="wikitable" style="border: 1px solid #D0E7FF; background-color:#ffffff; text-align:center;" border="1" | ||
|- | |- | ||
Line 64: | Line 99: | ||
|- | |- | ||
− | | bgcolor="#EAECF0" | <!-- INTENTIONALLY BLANK --> | + | | bgcolor="#EAECF0" |<!-- INTENTIONALLY BLANK --> |
! colspan="2" align="center" |'''[[Contact Alignment Recipes|<big>Contact Aligner Recipes</big>]]''' | ! colspan="2" align="center" |'''[[Contact Alignment Recipes|<big>Contact Aligner Recipes</big>]]''' | ||
! colspan="3" align="center" |'''[[Stepper Recipes|<big>Stepper Recipes</big>]]''' | ! colspan="3" align="center" |'''[[Stepper Recipes|<big>Stepper Recipes</big>]]''' | ||
− | ! align="center" | | + | ! align="center" |[[Direct-Write Lithography Recipes|Direct-Write Litho. Recipes]] |
|- | |- | ||
! width="150" bgcolor="#D0E7FF" align="center" |'''Positive Resists''' | ! width="150" bgcolor="#D0E7FF" align="center" |'''Positive Resists''' | ||
Line 78: | Line 113: | ||
|A | |A | ||
| | | | ||
− | | | + | |{{rl|MLA_Recipes|Positive Resist (MLA 150)}} |
|-<!-- This is a White row color --> | |-<!-- This is a White row color --> | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/f/fc/AXP4000pb-Datasheet.pdf AZ4210] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/f/fc/AXP4000pb-Datasheet.pdf AZ4210] | ||
Line 86: | Line 121: | ||
|A | |A | ||
| | | | ||
− | | | + | |A |
|- bgcolor="EEFFFF" | |- bgcolor="EEFFFF" | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/f/fc/AXP4000pb-Datasheet.pdf AZ4330RS] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/f/fc/AXP4000pb-Datasheet.pdf AZ4330RS] | ||
Line 94: | Line 129: | ||
|A | |A | ||
| | | | ||
− | | | + | |{{rl|MLA_Recipes|Positive Resist (MLA 150)}} |
|- | |- | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/a/a2/Az_p4620_photoresist_data_package.pdf AZ4620] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/a/a2/Az_p4620_photoresist_data_package.pdf AZ4620] | ||
− | | | + | |A |
− | | | + | |A |
− | | | + | |A |
− | | | + | |A |
| | | | ||
|A | |A | ||
|- bgcolor="EEFFFF" | |- bgcolor="EEFFFF" | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/8/8b/OCG825-Positive-Resist-Datasheet.pdf OCG 825-35CS] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/8/8b/OCG825-Positive-Resist-Datasheet.pdf OCG 825-35CS] | ||
− | | A | + | |A |
− | | A | + | |A |
− | | A | + | |A |
− | | A | + | |A |
− | |||
| | | | ||
+ | |A | ||
|- bgcolor="EEFFFF" | |- bgcolor="EEFFFF" | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/2/29/SPR955-Positive-Resist-Datasheet.pdf SPR 955 CM-0.9] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/2/29/SPR955-Positive-Resist-Datasheet.pdf SPR 955 CM-0.9] | ||
Line 118: | Line 153: | ||
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} | |{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} | ||
| | | | ||
− | | | + | |{{rl|MLA Recipes|Positive Resist (MLA 150)}} |
|- | |- | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/2/29/SPR955-Positive-Resist-Datasheet.pdf SPR 955 CM-1.8] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/2/29/SPR955-Positive-Resist-Datasheet.pdf SPR 955 CM-1.8] | ||
Line 126: | Line 161: | ||
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} | |{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} | ||
| | | | ||
− | | | + | |A |
|- bgcolor="EEFFFF" | |- bgcolor="EEFFFF" | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/3f/SPR220-Positive-Resist-Datasheet.pdf SPR 220-3.0] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/3f/SPR220-Positive-Resist-Datasheet.pdf SPR 220-3.0] | ||
Line 134: | Line 169: | ||
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} | |{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} | ||
| | | | ||
− | | | + | |{{rl|MLA Recipes|Positive Resist (MLA 150)}} |
|- | |- | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/3f/SPR220-Positive-Resist-Datasheet.pdf SPR 220-7.0] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/3f/SPR220-Positive-Resist-Datasheet.pdf SPR 220-7.0] | ||
Line 142: | Line 177: | ||
|{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} | |{{rl|Stepper Recipes|Positive Resist (AutoStep 200)}} | ||
| | | | ||
− | | | + | |A |
|- bgcolor="EEFFFF" | |- bgcolor="EEFFFF" | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/b/be/3600_D%2C_D2v_Spin_Speed_Curve.pdf THMR-IP3600 HP D] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/b/be/3600_D%2C_D2v_Spin_Speed_Curve.pdf THMR-IP3600 HP D] | ||
Line 150: | Line 185: | ||
|A | |A | ||
| | | | ||
− | | | + | |{{rl|MLA Recipes|Positive Resist (MLA 150)}} |
|- | |- | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/38/UV6-Positive-Resist-Datasheet.pdf UV6-0.8] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/38/UV6-Positive-Resist-Datasheet.pdf UV6-0.8] | ||
Line 185: | Line 220: | ||
|{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} | |{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} | ||
| | | | ||
− | | | + | |{{rl|MLA Recipes|Negative Resist (MLA 150)}} |
|- bgcolor="EEFFFF" | |- bgcolor="EEFFFF" | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/5/5e/AZnLOF2020-Negative-Resist-Datasheet.pdf AZnLOF 2020] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/5/5e/AZnLOF2020-Negative-Resist-Datasheet.pdf AZnLOF 2020] | ||
Line 193: | Line 228: | ||
|{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} | |{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} | ||
| | | | ||
− | | | + | |{{rl|MLA Recipes|Negative Resist (MLA 150)}} |
|- | |- | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/5/5e/AZnLOF2020-Negative-Resist-Datasheet.pdf AZnLOF 2035] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/5/5e/AZnLOF2020-Negative-Resist-Datasheet.pdf AZnLOF 2035] | ||
Line 201: | Line 236: | ||
| bgcolor="EEFFFF" |A | | bgcolor="EEFFFF" |A | ||
| bgcolor="EEFFFF" | | | bgcolor="EEFFFF" | | ||
− | | bgcolor="EEFFFF" | | + | | bgcolor="EEFFFF" |A |
|- bgcolor="EEFFFF" | |- bgcolor="EEFFFF" | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/5/5e/AZnLOF2020-Negative-Resist-Datasheet.pdf AZnLOF 2070] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/5/5e/AZnLOF2020-Negative-Resist-Datasheet.pdf AZnLOF 2070] | ||
Line 209: | Line 244: | ||
|A | |A | ||
| | | | ||
− | | | + | |A |
|- | |- | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/8/82/AZnLOF5510-Negative-Resist-Datasheet.pdf AZnLOF 5510] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/8/82/AZnLOF5510-Negative-Resist-Datasheet.pdf AZnLOF 5510] | ||
Line 217: | Line 252: | ||
|{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} | |{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} | ||
| | | | ||
− | | | + | |A |
|- bgcolor="EEFFFF" | |- bgcolor="EEFFFF" | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/c/c9/UVN-30_-_Negative-Resist-Datasheet_-_Apr_2004.pdf UVN30-0.8] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/c/c9/UVN-30_-_Negative-Resist-Datasheet_-_Apr_2004.pdf UVN30-0.8] | ||
Line 228: | Line 263: | ||
|- | |- | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/7/78/SU-8-2015-revA.pdf SU-8 2005,2010,2015] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/7/78/SU-8-2015-revA.pdf SU-8 2005,2010,2015] | ||
− | | A | + | |A |
− | | {{rl|Contact_Alignment_Recipes|Negative Resist (MA-6)}} | + | |{{rl|Contact_Alignment_Recipes|Negative Resist (MA-6)}} |
− | | A | + | |A |
− | | A | + | |A |
− | |||
| | | | ||
+ | |A | ||
|- bgcolor="EEFFFF" | |- bgcolor="EEFFFF" | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/2/2c/SU-8-2075-revA.pdf SU-8 2075] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/2/2c/SU-8-2075-revA.pdf SU-8 2075] | ||
Line 241: | Line 276: | ||
|A | |A | ||
| | | | ||
− | | | + | |{{rl|MLA Recipes|Negative Resist (MLA 150)}} |
|- | |- | ||
| bgcolor="#D0E7FF" align="center" |NR9-[//wiki.nanotech.ucsb.edu/w/images/8/8f/NR9-1000PY-revA.pdf 1000],[//wiki.nanotech.ucsb.edu/w/images/7/71/NR9-3000PY-revA.pdf 3000],[//wiki.nanotech.ucsb.edu/w/images/f/f9/NR9-6000PY-revA.pdf 6000]PY | | bgcolor="#D0E7FF" align="center" |NR9-[//wiki.nanotech.ucsb.edu/w/images/8/8f/NR9-1000PY-revA.pdf 1000],[//wiki.nanotech.ucsb.edu/w/images/7/71/NR9-3000PY-revA.pdf 3000],[//wiki.nanotech.ucsb.edu/w/images/f/f9/NR9-6000PY-revA.pdf 6000]PY | ||
Line 249: | Line 284: | ||
|{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} | |{{rl|Stepper Recipes|Negative Resist (AutoStep 200)}} | ||
| | | | ||
− | | | + | |A |
|- bgcolor="EEFFFF" | |- bgcolor="EEFFFF" | ||
− | ! bgcolor="#D0E7FF" align="center" | '''Anti-Reflection Coatings''' | + | ! bgcolor="#D0E7FF" align="center" |'''Anti-Reflection Coatings''' |
{{LithRecipe Table}} | {{LithRecipe Table}} | ||
|- | |- | ||
+ | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/3/33/XHRiC-Anti-Reflective-Coating.pdf XHRiC-11] | ||
+ | | | ||
+ | | | ||
+ | |A | ||
+ | |A | ||
+ | | | ||
+ | |A | ||
+ | |- bgcolor="EEFFFF" | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/0/07/DUV42P-Anti-Reflective-Coating.pdf DUV42-P] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/0/07/DUV42P-Anti-Reflective-Coating.pdf DUV42-P] | ||
| | | | ||
Line 259: | Line 302: | ||
| | | | ||
| | | | ||
− | |{{rl|Stepper Recipes|DUV-42P}} | + | |{{rl|Stepper Recipes|DUV-42P-6}} |
| | | | ||
− | |- | + | | |
+ | |- | ||
| bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/a/af/DS-K101-304-Anti-Reflective-Coating.pdf DS-K101-304] | | bgcolor="#D0E7FF" align="center" |[//wiki.nanotech.ucsb.edu/w/images/a/af/DS-K101-304-Anti-Reflective-Coating.pdf DS-K101-304] | ||
| | | | ||
Line 279: | Line 323: | ||
*{{fl|Liftoff-Techniques.pdf|Lift-Off Description/Tutorial}} | *{{fl|Liftoff-Techniques.pdf|Lift-Off Description/Tutorial}} | ||
**How it works, process limits and considerations for designing your process | **How it works, process limits and considerations for designing your process | ||
+ | *[[Lift-Off with I-Line Imaging Resist + LOL2000 Underlayer|I-Line Lift-Off: Bi-Layer Process with LOL2000 Underlayer]] | ||
+ | **''Single Expose/Develop process for simplicity'' | ||
+ | **''Up to ~130nm metal thickness & ≥500nm-1000nm gap between metal.'' | ||
+ | **''Can use any I-Line litho tool (GCA Stepper, Contact aligner, MLA)'' | ||
*{{fl|Bi-LayerContactprocesswithPMGI.pdf|I-Line Lift-Off: Bi-Layer Process with PMGI Underlayer and Contact Aligner}} | *{{fl|Bi-LayerContactprocesswithPMGI.pdf|I-Line Lift-Off: Bi-Layer Process with PMGI Underlayer and Contact Aligner}} | ||
+ | **''Multiple processes for Metal thicknesses ~800nm to ~2.5µm'' | ||
+ | **''Uses multiple DUV Flood exposure/develop cycles to create undercut.'' | ||
+ | **''Can be transferred to other I-Line litho tools (Stepper, MLA etc.)'' | ||
*[[Lift-Off with DUV Imaging + PMGI Underlayer|DUV Lift-Off: UV6 Imaging Resist + PMGI Underlayer]] | *[[Lift-Off with DUV Imaging + PMGI Underlayer|DUV Lift-Off: UV6 Imaging Resist + PMGI Underlayer]] | ||
+ | **''Single-expose/develop process'' | ||
+ | **''Up to ~65nm metal thickness & ~350nm gap between metal'' | ||
+ | **''Use thicker PMGI for thicker metals'' | ||
==[[E-Beam Lithography System (JEOL JBX-6300FS)|E-Beam Lithography Recipes (JEOL JBX-6300FS)]]== | ==[[E-Beam Lithography System (JEOL JBX-6300FS)|E-Beam Lithography Recipes (JEOL JBX-6300FS)]]== | ||
Line 286: | Line 340: | ||
*Under Development. | *Under Development. | ||
− | == [[Focused Ion-Beam Lithography (Raith Velion)|FIB Lithography Recipes (Raith Velion)]] == | + | ==[[Focused Ion-Beam Lithography (Raith Velion)|FIB Lithography Recipes (Raith Velion)]]== |
''To Be Added'' | ''To Be Added'' | ||
==[[Automated Coat/Develop System (S-Cubed Flexi)|Automated Coat/Develop System Recipes (S-Cubed Flexi)]]== | ==[[Automated Coat/Develop System (S-Cubed Flexi)|Automated Coat/Develop System Recipes (S-Cubed Flexi)]]== | ||
Recipes pre-loaded on the S-Cubed Flexi automated coat/bake/develop system. Only staff may write new recipes, contact the tool supervisor for more info. | Recipes pre-loaded on the S-Cubed Flexi automated coat/bake/develop system. Only staff may write new recipes, contact the tool supervisor for more info. | ||
+ | {| class="wikitable" | ||
+ | |+''Ask [[Tony Bosch|Staff]] if you need a new recipe.'' | ||
+ | |'''''<u>Coating Material</u>''''' | ||
+ | |'''''<u>Route/Chain</u>''''' | ||
+ | |'''''<u>Name</u>''': User: "UCSB Users"'' | ||
+ | |'''''<u>Spin Speed (krpm)</u>''''' | ||
+ | |'''''<u>Bake Temp</u>''''' | ||
+ | |'''''<u>Notes</u>''''' | ||
+ | |- | ||
+ | |'''''DS-K101''''' | ||
+ | |''Route'' | ||
+ | | colspan="4" |''DSK101's Develop Rate depends on Bake temp - you can use this to control undercut.'' | ||
− | '' | + | ''See: [[DS-K101-304 Bake Temp. versus Develop Rate|DSK Bake vs. Dev rate]]'' |
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-220C | ||
+ | |5.0 | ||
+ | |220°C | ||
+ | |''Requires: HP4=220°C'' | ||
+ | This is essentailly equivalent to [[Stepper Recipes#DUV-42P-6|DUV42P @ 220°C]], must be dry etched. | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-210C | ||
+ | |5.0 | ||
+ | |210°C | ||
+ | |''Requires: HP4=210°C'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-200C | ||
+ | |5.0 | ||
+ | |200°C | ||
+ | |''Requires: HP4=200°C'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-185C | ||
+ | |5.0 | ||
+ | |185°C | ||
+ | |''Requires: HP4=185°C'' | ||
+ | |- | ||
+ | |'''''UV6-0.8''''' | ||
+ | |''Route'' | ||
+ | |Coat-UV6[2K]-135C | ||
+ | |2.0 | ||
+ | |135°C | ||
+ | |''Requires: HP1=135°C'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-UV6[2.5K]-135C | ||
+ | |2.5 | ||
+ | |135°C | ||
+ | | | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-UV6[3K]-135C | ||
+ | |3.0 | ||
+ | |135°C | ||
+ | | | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-UV6[3.5K]-135C | ||
+ | |3.5 | ||
+ | |135°C | ||
+ | | | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-UV6[4K]-135C | ||
+ | |4.0 | ||
+ | |135°C | ||
+ | | | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-UV6[5K]-135C | ||
+ | |5.0 | ||
+ | |135°C | ||
+ | | | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-UV6[6K]-135C | ||
+ | |6.0 | ||
+ | |135°C | ||
+ | | | ||
+ | |- | ||
+ | |'''''DS-K101 @ 220°C''''' | ||
+ | '''''+ UV6''''' | ||
+ | |''Chain'' | ||
+ | |Coat-DSK101[5K]-220C-UV6[2K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 2.0krpm'' | ||
+ | |DSK: 220°C | ||
+ | UV6: 135°C | ||
+ | |''Requires:'' | ||
+ | ''– HP4=220°C'' | ||
− | = | + | ''– HP1=135°C'' |
− | + | ''Plan for ~10-15 min per wafer.'' | |
− | + | |- | |
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-220C-UV6[2.5K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 2.5krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-220C-UV6[3K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 3.0krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-220C-UV6[3.5K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 3.5krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-220C-UV6[4K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 4.0krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-220C-UV6[5K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 5.0krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-220C-UV6[6K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 6.0krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | |'''''DS-K101 @ 185°C''''' | ||
+ | '''''+ UV6''''' | ||
+ | |''Chain'' | ||
+ | |Coat-DSK101[5K]-185C-UV6[2K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 2.0krpm'' | ||
+ | |DSK: 185°C | ||
+ | UV6: 135°C | ||
+ | |''Requires:'' | ||
+ | ''– HP4=185°C'' | ||
+ | ''– HP1=135°C'' | ||
+ | |||
+ | ''Plan for ~10-15 min per wafer.'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-185C-UV6[2.5K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 2.5krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-185C-UV6[3K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 3.0krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-185C-UV6[3.5K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 3.5krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-185C-UV6[4K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 4.0krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-185C-UV6[5K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 5.0krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |Coat-DSK101[5K]-185C-UV6[6K]-135C | ||
+ | |''DSK: 5krpm'' | ||
+ | ''UV6: 6.0krpm'' | ||
+ | |''same as above'' | ||
+ | |''same as above'' | ||
+ | |- | ||
+ | |'''''Hotplate Set''''' | ||
+ | |''Route'' | ||
+ | |''SET-HP4-220C'' | ||
+ | | | ||
+ | |220°C | ||
+ | |''Hotplate 4 (top) between 218-222°C when done.'' | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |''SET-HP4-210C'' | ||
+ | | | ||
+ | |210°C | ||
+ | | | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |''SET-HP4-200C'' | ||
+ | | | ||
+ | |200°C | ||
+ | | | ||
+ | |- | ||
+ | | | ||
+ | | | ||
+ | |''SET-HP4-185C'' | ||
+ | | | ||
+ | |185*C | ||
+ | | | ||
+ | |} | ||
==[[Holographic Lith/PL Setup (Custom)|Holography Recipes]]== | ==[[Holographic Lith/PL Setup (Custom)|Holography Recipes]]== | ||
+ | ''The Holography recipes here use the BARC layer XHRiC-11 & the high-res. I-Line photoresist THMR-IP3600HP-D.'' | ||
− | *{{fl|Holography_Process_for_1D-lines_and_2D-dots_ | + | *{{fl|Holography_Process_for_1D-lines_and_2D-dots_%28ARC-11_%26_THMR-IP3600HP-D%29-updated-4-8-2021.pdf|Standard Holography Process - on SiO2 on Si}} |
*{{fl|Holography-Process-Variation-revA.pdf|Holography Process Variations - Set-up Angle - Etching into SiO2 and Si}} | *{{fl|Holography-Process-Variation-revA.pdf|Holography Process Variations - Set-up Angle - Etching into SiO2 and Si}} | ||
*{{fl|05-SiO2_Nano-structure_Etch.pdf|Etch SiO2 Nano-structure - Changing Side-wall Angle - Etching into Si with a different line-width}} | *{{fl|05-SiO2_Nano-structure_Etch.pdf|Etch SiO2 Nano-structure - Changing Side-wall Angle - Etching into Si with a different line-width}} | ||
Line 322: | Line 616: | ||
*{{fl|AXP4000pb-Datasheet.pdf|AZP4000 (AZ4110, AZ4210, AZ4330)}} | *{{fl|AXP4000pb-Datasheet.pdf|AZP4000 (AZ4110, AZ4210, AZ4330)}} | ||
+ | *{{Fl|Az_p4620_photoresist_data_package.pdf|AZ P4620}} | ||
*{{fl|OCG825-Positive-Resist-Datasheet.pdf|OCG825}} | *{{fl|OCG825-Positive-Resist-Datasheet.pdf|OCG825}} | ||
*{{fl|SPR220-Positive-Resist-Datasheet.pdf|SPR220 (SPR220-3, SPR220-7)}} | *{{fl|SPR220-Positive-Resist-Datasheet.pdf|SPR220 (SPR220-3, SPR220-7)}} | ||
Line 378: | Line 673: | ||
*{{fl|XHRiC-Anti-Reflective-Coating.pdf|XHRiC-11 (i-line)}} | *{{fl|XHRiC-Anti-Reflective-Coating.pdf|XHRiC-11 (i-line)}} | ||
− | *{{fl|DUV42P-Anti-Reflective-Coating.pdf|DUV42P (DUV) (For AR2 replacement)}} | + | *{{fl|DUV42P-Anti-Reflective-Coating.pdf|DUV42P-6 (DUV) (For AR2 replacement)}} |
*{{fl|DS-K101-304-Anti-Reflective-Coating.pdf|DS-K101-304 (DUV developable BARC)}} | *{{fl|DS-K101-304-Anti-Reflective-Coating.pdf|DS-K101-304 (DUV developable BARC)}} | ||
Latest revision as of 21:43, 16 February 2023
Table of Contents |
---|
Photolithography Processes
|
Photolithography Chemicals/Materials
|
General Photolithography Techniques
HMDS Process for Improving Adhesion
- Use these procedures if you are finding poor adhesion PR lifting-off), or for chemicals (like BHF) that attack the PR adhesion interface strongly.
Edge-Bead Removal Techniques
- These techniques are required for loading full-wafers into etchers that use top-side clamps, to prevent photoresist from sticking to the clamp (and potentially destroying your wafer).
- For contact lithography, this improves the proximity of the mask plate and sample, improving resolution. For some projection systems, such as the Maskless Aligner, EBR can help with autofocus issues.
Photoresist reflow (MicroChem)
- To create slanted sidewalls or curved surfaces.
Photolithography Recipes
- R: Recipe is available. Clicking this link will take you to the recipe.
- A: Material is available for use, but no recipes are provided.
Click the tool title to go to recipes for that tool.
Click the photoresist title to get the datasheet, also found in Stocked Chemicals + Datasheets.
Lift-Off Recipes
- Lift-Off Description/Tutorial
- How it works, process limits and considerations for designing your process
- I-Line Lift-Off: Bi-Layer Process with LOL2000 Underlayer
- Single Expose/Develop process for simplicity
- Up to ~130nm metal thickness & ≥500nm-1000nm gap between metal.
- Can use any I-Line litho tool (GCA Stepper, Contact aligner, MLA)
- I-Line Lift-Off: Bi-Layer Process with PMGI Underlayer and Contact Aligner
- Multiple processes for Metal thicknesses ~800nm to ~2.5µm
- Uses multiple DUV Flood exposure/develop cycles to create undercut.
- Can be transferred to other I-Line litho tools (Stepper, MLA etc.)
- DUV Lift-Off: UV6 Imaging Resist + PMGI Underlayer
- Single-expose/develop process
- Up to ~65nm metal thickness & ~350nm gap between metal
- Use thicker PMGI for thicker metals
E-Beam Lithography Recipes (JEOL JBX-6300FS)
- Under Development.
FIB Lithography Recipes (Raith Velion)
To Be Added
Automated Coat/Develop System Recipes (S-Cubed Flexi)
Recipes pre-loaded on the S-Cubed Flexi automated coat/bake/develop system. Only staff may write new recipes, contact the tool supervisor for more info.
Coating Material | Route/Chain | Name: User: "UCSB Users" | Spin Speed (krpm) | Bake Temp | Notes |
DS-K101 | Route | DSK101's Develop Rate depends on Bake temp - you can use this to control undercut. | |||
Coat-DSK101[5K]-220C | 5.0 | 220°C | Requires: HP4=220°C
This is essentailly equivalent to DUV42P @ 220°C, must be dry etched. | ||
Coat-DSK101[5K]-210C | 5.0 | 210°C | Requires: HP4=210°C | ||
Coat-DSK101[5K]-200C | 5.0 | 200°C | Requires: HP4=200°C | ||
Coat-DSK101[5K]-185C | 5.0 | 185°C | Requires: HP4=185°C | ||
UV6-0.8 | Route | Coat-UV6[2K]-135C | 2.0 | 135°C | Requires: HP1=135°C |
Coat-UV6[2.5K]-135C | 2.5 | 135°C | |||
Coat-UV6[3K]-135C | 3.0 | 135°C | |||
Coat-UV6[3.5K]-135C | 3.5 | 135°C | |||
Coat-UV6[4K]-135C | 4.0 | 135°C | |||
Coat-UV6[5K]-135C | 5.0 | 135°C | |||
Coat-UV6[6K]-135C | 6.0 | 135°C | |||
DS-K101 @ 220°C
+ UV6 |
Chain | Coat-DSK101[5K]-220C-UV6[2K]-135C | DSK: 5krpm
UV6: 2.0krpm |
DSK: 220°C
UV6: 135°C |
Requires:
– HP4=220°C – HP1=135°C Plan for ~10-15 min per wafer. |
Coat-DSK101[5K]-220C-UV6[2.5K]-135C | DSK: 5krpm
UV6: 2.5krpm |
same as above | same as above | ||
Coat-DSK101[5K]-220C-UV6[3K]-135C | DSK: 5krpm
UV6: 3.0krpm |
same as above | same as above | ||
Coat-DSK101[5K]-220C-UV6[3.5K]-135C | DSK: 5krpm
UV6: 3.5krpm |
same as above | same as above | ||
Coat-DSK101[5K]-220C-UV6[4K]-135C | DSK: 5krpm
UV6: 4.0krpm |
same as above | same as above | ||
Coat-DSK101[5K]-220C-UV6[5K]-135C | DSK: 5krpm
UV6: 5.0krpm |
same as above | same as above | ||
Coat-DSK101[5K]-220C-UV6[6K]-135C | DSK: 5krpm
UV6: 6.0krpm |
same as above | same as above | ||
DS-K101 @ 185°C
+ UV6 |
Chain | Coat-DSK101[5K]-185C-UV6[2K]-135C | DSK: 5krpm
UV6: 2.0krpm |
DSK: 185°C
UV6: 135°C |
Requires:
– HP4=185°C – HP1=135°C Plan for ~10-15 min per wafer. |
Coat-DSK101[5K]-185C-UV6[2.5K]-135C | DSK: 5krpm
UV6: 2.5krpm |
same as above | same as above | ||
Coat-DSK101[5K]-185C-UV6[3K]-135C | DSK: 5krpm
UV6: 3.0krpm |
same as above | same as above | ||
Coat-DSK101[5K]-185C-UV6[3.5K]-135C | DSK: 5krpm
UV6: 3.5krpm |
same as above | same as above | ||
Coat-DSK101[5K]-185C-UV6[4K]-135C | DSK: 5krpm
UV6: 4.0krpm |
same as above | same as above | ||
Coat-DSK101[5K]-185C-UV6[5K]-135C | DSK: 5krpm
UV6: 5.0krpm |
same as above | same as above | ||
Coat-DSK101[5K]-185C-UV6[6K]-135C | DSK: 5krpm
UV6: 6.0krpm |
same as above | same as above | ||
Hotplate Set | Route | SET-HP4-220C | 220°C | Hotplate 4 (top) between 218-222°C when done. | |
SET-HP4-210C | 210°C | ||||
SET-HP4-200C | 200°C | ||||
SET-HP4-185C | 185*C |
Holography Recipes
The Holography recipes here use the BARC layer XHRiC-11 & the high-res. I-Line photoresist THMR-IP3600HP-D.
- Standard Holography Process - on SiO2 on Si
- Holography Process Variations - Set-up Angle - Etching into SiO2 and Si
- Etch SiO2 Nano-structure - Changing Side-wall Angle - Etching into Si with a different line-width
- Reduce SiO2 Nanowire Diameter - Thermal Oxidation - Vapor HF Etching
Low-K Spin-On Dielectric Recipes
Chemicals Stocked + Datasheets
The following is a list of the lithography chemicals we stock in the lab, with links to the datasheets for each. The datasheets will often have important processing info such as spin-speed vs. thickness curves, typical process parameters, bake temps/times etc.